MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Makrolon® LF sheet Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: Low flammability Makrolon® LF sheet is a flame resistant, UV stabilized, transparent polycarbonate product. It features a UL 94 V-0 rating and meets FAR 25.853 (a), 1, (i) requirements at 0.080 in. and thicker. The product offers high impact strength, superior dimensional stability, high temperature resistance, and high clarity. This lightweight thermoformable sheet is also easy to fabricate and decorate.

Applications: Electrical devices, equipment housings, switchgear covers, light fixtures

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 65.5 MPaASTM D638
Modulus of Elasticity 2.34 GPaASTM D638
Flexural Strength 93.1 MPaASTM D790
Compressive Strength 86.2 MPaASTM D695
Izod Impact, Notched 15.0 ft-lb/in
@Thickness 3.17 mm
ASTM D256
Izod Impact, Unnotched 60.0 ft-lb/in
@Thickness 3.17 mm
no failure; ASTM D256
Impact Test >= 46.0 ft-lb
@Thickness 3.17 mm
ASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear 37.5 µin/in-°FASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 142 °CASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 132 °CASTM D648
Flammability, UL94 V-0
@Thickness 2.03 mm
 
Optical PropertiesOriginal ValueComments
Haze <= 1.0 %ASTM D10003
Transmission, Visible 86 %
@Thickness 3.00 mm
ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Makrolon® GP-V sheet Polycarbonate
Overview of materials for Nylon 66/6, 30% Glass Fiber Reinforced
Covestro Makrolon® GP-V Matte sheet Polycarbonate
Covestro Makrolon® 2256 Polycarbonate
Overview of materials for Polyphenylene Sulfide (PPS); Molded

PCOVEST0839 / 202622

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.