MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
CHT Group QSil 217 Transparent, Liquid Silicone Rubber
Categories: Polymer; Thermoset; Silicone; Silicone Rubber; Liquid Silicone Rubber (LSR)

Material Notes: Product Description: QSil 217 is a two-part, clear, liquid silicone that will cure at room temperature or at elevated temperatures. It has a low viscosity, which allows for ease of flow around complex parts, providing electrical insulation and shock resistance. The chemical composition provides hydrolytic and reversion resistance.

Key Features:

  • Convenient 1:1 mixing ratio for use in automatic dispensing equipment or hand mixing
  • Contains no solvents
  • Non-yellowing catalyst system

Formerly Amber Chemical Co (ACC Silicones), aquired by CHT in 2017

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.970 g/ccUncatalyzed, QSil 217A
 0.970 g/ccUncatalyzed, QSil 217B
Viscosity 300 cPUncatalyzed, QSil 217B
 360 cPUncatalyzed, QSil 217A
Linear Mold Shrinkage <= 0.0010 cm/cmCured 60 minutes @ 100°C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 35Cured 60 minutes @ 100°C
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cm
Dielectric Constant 3.0
@Frequency 1000 Hz
Dielectric Strength 18.9 kV/mm
Dissipation Factor 0.0020
@Frequency 1000 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 280 µm/m-°C
Specific Heat Capacity 0.700 J/g-°C
Thermal Conductivity 0.180 W/m-K
Maximum Service Temperature, Air 204 °C
Minimum Service Temperature, Air -55.0 °C
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.406Cured 60 minutes @ 100°C
 
Processing PropertiesOriginal ValueComments
Cure Time 60.0 min
@Temperature 100 °C
As Tested
Gel Time 20.0 minCatalyzed
 
Descriptive Properties
ColorClearUncatalyzed, QSil 217A
 ClearUncatalyzed, QSil 217B
 Clear, colorlessCatalyzed

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Silicone Rubber
CHT Group QSil 213 Transparent, Liquid Silicone Rubber
CHT Group QSil 218 Transparent, Liquid Silicone Rubber
CHT Group QSil 220 Transparent, Liquid Silicone Rubber
CHT Group QSil 219 Transparent, Liquid Silicone Rubber

PACC2081 / 199469

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.