MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Selar® PT 4274 Polyester Barrier Resin  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyester Film

Material Notes: Selar® PT 4274 is a toughened homopolymer polyester resin in the high melt viscosity (HMV) series designed for thermoplastic processes. The HMV modification changes the rheology of the melt and provides better processibility in extrusion operations. It can be processed in conventional extruders designed for polyolefins or polyesters.

Information provided by DuPont Packaging Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.30 g/ccASTM D1505
Moisture Vapor Transmission 1.20 cc-mm/m²-24hr-atm
Oxygen Transmission 4.90 cc-mm/m²-24hr-atm
Viscosity 800000 cP
@Shear Rate 100 1/s,
Temperature 270 °C
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 35.2 MPaASTM D882
Film Tensile Strength at Yield, TD 27.6 MPaASTM D882
Film Elongation at Break, MD 440 %ASTM D882
Film Elongation at Break, TD 445 %ASTM D882
Secant Modulus, MD 1.72 GPaASTM D882
Secant Modulus, TD 1.76 GPaASTM D882
Impact 5.2J/mm Spencer Impact; ASTM D3420
Coefficient of Friction 0.20film/metal; ASTM D1894
Graves Tear Strength 219 kN/mTD; ASTM D1004
 233 kN/mMD; ASTM D1004
Elmendorf Tear Strength, MD 21.0 g/mil50 µm (2 mil) film; ASTM D1922
Elmendorf Tear Strength, TD 22.0 g/mil50 µm (2 mil) film; ASTM D1922
Seal Strength 3000 g/25 mmseal bar 149°C.
Film Tensile Strength at Break, MD 41.0 MPaASTM D882
Film Tensile Strength at Break, TD 41.0 MPaASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 255 °CDSC/ASTM D3418
Glass Transition Temp, Tg 75.0 °CASTM D3418
 
Processing PropertiesOriginal ValueComments
Melt Temperature 268 - 279 °C
Drying Temperature 121 - 135 °C
Dry Time 6 - 8 hourto < 0.005% moisture.

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Selar® PT 8307 Polyester Barrier Resin
Overview of materials for Polyester Thermoplastic Elastomer
DuPont Teijin Films Mylar® 50 M44E Polyester Film, One-Sided PVDC Barrier Coated, 50 Gauge
Michelman® Topaz Indicator Solution
Topaz, Al2SiO3(OH,F)2

PDUPL2 / 33658

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.