MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ascend Performance Materials Starflam® 315J NT0725 PA66/6 FR
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, Unreinforced

Material Notes: Starflam 315J NT0725 (formerly Vydyne® ECO315J NT0725) is a non-halogenated, unreinforced, flame-retardant PA66/6 co-polymer compound designed with high ductility (20% elongation), high comparative tracking index (CTI), and low corrosion for improved electrical contact performance. It is stabilized to provide heat stability up to 125°C for 1,000 hours in a dry environment. It exhibits excellent toughness and ductility, allowing increased flexibility in product design needed for living hinges and snap fits. 315J NT0725 provides enhanced flow and is lubricated for machine feed and easy mold release.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.16 g/ccDAM; ISO 1183
Water Absorption 0.80 %
@Time 86400 sec
DAM; ISO 62
Moisture Absorption at Equilibrium 2.3 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.012 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.014 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 42.0 MPa50% RH; ISO 527-2
 75.0 MPaDAM; ISO 527-2
Elongation at Break 22 %DAM; ISO 527-2
 140 %50% RH; ISO 527-2
Elongation at Yield 3.5 %DAM; ISO 527-2
 23 %50% RH; ISO 527-2
Tensile Modulus 1200 MPa50% RH; ISO 527-2
 3200 MPaDAM; ISO 527-2
Flexural Strength 45.0 MPa50% RH; ISO 178
 92.0 MPaDAM; ISO 178
Flexural Modulus 1600 MPa50% RH; ISO 178
 3200 MPaDAM; ISO 178
Poissons Ratio 0.40ISO 527-2
Izod Impact, Notched (ISO) 5.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 5.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 6.00 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 13.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched NB
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature -30.0 °C
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 4.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 5.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 15.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+11 ohm-cm
@Thickness 1.00 mm
DAM; IEC 60093
Dielectric Strength 13.0 kV/mm
@Thickness 1.00 mm
DAM; IEC 60243
Arc Resistance 120 - 180 sec
@Thickness 3.00 mm
PLC 5; ASTM D 495
Comparative Tracking Index 600 V
@Thickness 3.00 mm
IEC 60112
Hot Wire Ignition, HWI 7.0 - 15 secPLC 4; UL 746
 7.0 - 15 secPLC 4; UL 746
 7.0 - 15 secPLC 4; UL 746
 15 - 30 secPLC 3; UL 746
High Amp Arc Ignition, HAI >= 120 arcsPLC 0; UL 746
 >= 120 arcsPLC 0; UL 746
 >= 120 arcsPLC 0; UL 746
 >= 120 arcsPLC 0; UL 746
High Voltage Arc-Tracking Rate, HVTR 10.0 - 25.4 mm/minPLC 1; UL 746
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 110 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 110 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
DAM; ISO 11359-2
Melting Point 244 °CDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 225 °CUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °CUnannealed; DAM; ISO 75-2/A
UL RTI, Electrical 130 °C
@Thickness 0.400 mm
UL 746
 130 °C
@Thickness 0.750 mm
UL 746
 130 °C
@Thickness 1.50 mm
UL 746
 130 °C
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical with Impact 65.0 °C
@Thickness 0.400 mm
UL 746
 65.0 °C
@Thickness 0.750 mm
UL 746
 85.0 °C
@Thickness 1.50 mm
UL 746
 85.0 °C
@Thickness 3.00 mm
UL 746
UL RTI, Mechanical without Impact 100 °C
@Thickness 0.400 mm
UL 746
 100 °C
@Thickness 0.750 mm
UL 746
 100 °C
@Thickness 1.50 mm
UL 746
 110 °C
@Thickness 3.00 mm
UL 746
Flammability, UL94 V-0
@Thickness 0.400 mm
 V-0
@Thickness 0.750 mm
 V-0
@Thickness 1.50 mm
 V-0
@Thickness 3.00 mm
Oxygen Index 29 %DAM; EN ISO 4589-2
Glow Wire Ignition Temperature 725 °C
@Thickness 3.00 mm
IEC 60695-2-13
 775 °C
@Thickness 1.50 mm
IEC 60695-2-13
 875 °C
@Thickness 0.400 mm
IEC 60695-2-13
 875 °C
@Thickness 0.750 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 0.400 mm
IEC 60695-2-12
 960 °C
@Thickness 0.750 mm
IEC 60695-2-12
 960 °C
@Thickness 1.50 mm
IEC 60695-2-12
 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 240 - 270 °CInjection
Middle Barrel Temperature 240 - 270 °CInjection
Front Barrel Temperature 240 - 270 °CInjection
Nozzle Temperature 240 - 270 °CInjection
Melt Temperature 250 - 270 °CInjection
Mold Temperature 65.0 - 95.0 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 4.00 hourInjection
 
Descriptive Properties
AdditiveFlame Retarding Agent
 Heat Stabilizer
 Lubricant
AppearanceNatural Color
FeaturesCrack Resistant
 Ductile
 Flame Retardant
 Good Mold Release
 Good Toughness
 Halogen Content, None
 High Elongation
 Low Density
 Lubricated
 Organic Heat Stabilized
FormsPellets
Processing MethodInjection Molding
RegionNorth America, Europe, Asia Pacific
UL File NumberE70062

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PASCE9103 / 287554

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.