MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 977-2 Epoxy - Carbon Fiber Laminate
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: CYCOM® 977-2 is a 350°F (177°C) curing toughened epoxy resin with a 260 – 280°F (126 – 138°C) dry and 220°F (104°C) wet service capability. CYCOM 977-2 is formulated for autoclave or press molding. Unidirectional tape and woven fabric impregnated with CYCOM 977-2 resin will retain tack for at least 10 days at 72°F (22°C) and has a long mechanical out life suitable for fabrication of large structures. The recommended lay-up procedure for this material is L-15. The recommended cure is C-50.

Features & Benefits:

  • Toughened epoxy using Cytec Engineered Materials’ proprietary “co-continuous” morphology
  • 350°F (177°C) cure
  • Available in a broad range of fibers and forms including tape, fabric and roving
  • Excellent impact resistance
  • Controlled flow
  • 260 – 280°F (126 – 138°C) dry and 220°F (104°C) wet service temperature
  • Autoclave or press mold processing
  • Shelf life of 12 months at 0°F (-18°C), 42 days at 72°F (22°C)
Applications:
  • Aircraft primary and secondary structure
  • Space structure
  • Ballistics
  • Cryogenic tanks
  • Any application where impact resistance and light weight are required
Mechanical property data per BMS 8-276 for epoxy laminate with 57-63% fiber volume Intermediate Modulus [40 msi (276 GPa) Class] Carbon Fiber Reinforced Unidirectional Tape. 'Wet' property data after 7 day water immersion at 165°F (74°C).

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 65000 psiQuasi Open Hole
 390000 psi
@Temperature -55.0 °C
 390000 psi
@Temperature 24.0 °C
Tensile Modulus 165 GPa
@Temperature -55.0 °C
 165 GPa
@Temperature 24.0 °C
Flexural Strength 27600 - 29600 psiNeat Resin
Flexural Modulus 3.38 - 3.52 GPaNeat Resin
Compressive Strength 255 MPa
@Temperature 82.0 °C
Quasi Open Hole, wet
 262 MPa
@Temperature 24.0 °C
Quasi After 1500 in-lb/in Impact
 269 MPa
@Temperature 82.0 °C
Quasi Open Hole
 310 MPa
@Temperature 24.0 °C
Quasi Open Hole
 1240 MPa
@Temperature 82.0 °C
0°, wet
 1450 MPa
@Temperature 82.0 °C
 1580 MPa
@Temperature 24.0 °C
Compressive Modulus 152000 MPa
@Temperature 24.0 °C
 152000 MPa
@Temperature 82.0 °C
 152000 MPa
@Temperature 82.0 °C
0°, wet
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 104 °Cwet
 138 °Cdry
Glass Transition Temp, Tg 212 °CNeat Resin
 
Processing PropertiesOriginal ValueComments
Processing Temperature 355 °F
@Time 10800 sec
Cure

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 5320-1 Epoxy with T40/800B Unidirectional Tape Composite
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with IM7-6K-4HS Fabric
Solvay CYCOM® 5250-4 RTM BMI Resin, Composite with T650-35-3K-PW Fabric
Solvay CYCOM® 890 RTM Resin - Woven Carbon Fabric Composite
Solvay CYCOM® 977-3 Epoxy - Unidirectional Carbon Fiber Tape

PCYTED089a / 234744

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.