MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Chemically Resistant adhesives

(Viewing data as-entered. Click here to return)
Lord Adhesives CoolTherm™ SC-420 Thermally Conductive Silicone Encapsulant System
Categories: Polymer; Thermoset; Silicone; Silicone Elastomer, for Thermal Management

Material Notes: LORD CoolTherm™ SC-420 thermally conductive silicone encapsulant is a two-component system designed to provide excellent thermal conductivity and flexibility for electrical/electronic encapsulating applications, while retaining desirable properties associated with silicones. CoolTherm SC-420 hardener evolves minute quantities of hydrogen gas. Do not repackage or store material in unvented containers. Adequately ventilate work area to prevent the accumulation of gas.

Features: exhibits low shrinkage and stress on components as it cures. composed of an addition-curing polydimethyl siloxane polymer that will not depolymerize when heated in confined spaces. maintains low viscosity for ease of component encapsulation compared to other highly thermally conductive materials. provides excellent thermal shock resistance.

All information provided by Lord.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 3.18 g/ccSC-420 Resin
 3.18 g/ccSC-420 Hardener
 3.18 g/ccMixed
Water Absorption <= 0.50 %cured; ASTM D 570-81
Viscosity 27000 cP
@Temperature 25.0 °C
SC-420 Hardener
 50000 cP
@Temperature 25.0 °C
Mixed
 63000 cP
@Temperature 25.0 °C
SC-420 Resin
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 20cured; ASTM D 2240
Tensile Strength 145 psicured; ASTM D412
Elongation at Break 100 %cured; ASTM D 412
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 ohm-cm
@Temperature 25.0 °C
cured; ASTM D 257
 
Thermal PropertiesOriginal ValueComments
CTE, linear 100 µm/m-°Ccured; ASTM C 864
Thermal Conductivity 3.20 W/m-Kcured, hot disc transient method
 
Processing PropertiesOriginal ValueComments
Pot Life >= 30.0 min
@Temperature 25.0 °C
mixed
Gel Time 70.0 min
@Temperature 25.0 °C
mixed
Shelf Life 9.00 Month
@Temperature 25.0 °C
each component, from date of manufacture when stored in original, unopened container
 
Descriptive Properties
AppearanceBlack PasteSC-420 Resin
 Grey PasteMixed
 White PasteSC-420 Hardener

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lord Adhesives CoolTherm™ SC-324 Thermally Conductive Epoxy Encapsulant
Lord Adhesives CoolTherm™ SC-322 Thermally Conductive Adhesive
Lord Adhesives CoolTherm™ SC-320 THK Thermally Conductive Silicone
Lord Adhesives CoolTherm™ SC-320 Thermally Conductive Silicone Encapsulant
Lord Adhesives CoolTherm™ SC-320 SLW Thermally Conductive Silicone Encapsulant

PLORD9253 / 232609

Chemically Resistant adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.