MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay CYCOM® E773 and E773FR Epoxy Neat Resin
Categories: Polymer; Thermoset; Epoxy

Material Notes: CYCOM® E773/E773FR resins are controlled flow epoxy systems with a large processing window. They exhibit excellent high temperature performance up to 180°F (82°C) wet service temperature. The systems have good retention of tack and drape up to 20 days at room temperature in prepreg form. A straight two hour ramp cure in either a press or an autoclave may be used. No post-cure is requirement to achieve service temperature.

Features & Benefits:

  • 250°F (121°C) cure
  • 180°F (82°C) wet service temperature
  • Low exotherm profile
  • Controlled flow
  • Large processing window
  • Available in both flame retardant (FR) and non-flame retardant grades
  • Autoclave or press mold processing
  • Available in unidirectional tape, fabric, roving, slit tape and cross-plied forms
  • History of performance on helicopter blades and other structural components
  • Shelf life of 12 months at 0°F (-18°C), 20 days at 72°F (22°C)
Applications:
  • Helicopter blades
  • Other aircraft structural components

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.28 g/ccDry
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 9300 psiDry
Tensile Modulus 3.50 GPaDry
Flexural Strength 13600 psiDry
Flexural Modulus 3.80 GPaDry
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 180 °Fwet service
Glass Transition Temp, Tg 115 °Cwet (90 hour water soak at 160°F (71°C)
 155 °Cdry
 
Processing PropertiesOriginal ValueComments
Processing Temperature 260 °F
@Time 5400 sec
plus ramp up and cooldown
Shelf Life 0.667 Month
@Temperature 22.2 °C
 12.0 Month
@Temperature -17.8 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Norplex-Micarta NorPLY™ 1002 Epoxy Fiberglass Composite, Unidirectional
Solvay CYCOM® 977-6 Epoxy Laminate with IM7 Unidirectional Tape
Norplex-Micarta NorPLY™ 1002 Epoxy Fiberglass Composite, Crossply
Solvay CYCOM® 5216 Epoxy - Unidirectional S-Glass Prepreg, After Environmental Exposure
Solvay CYCOM® 5216 Epoxy - Woven Aramid Fiber Prepreg

PCYTED100 / 180402

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.