MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Aluminum 2618-T61
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92618; Aluminium 2618-T61; AA2618-T61; Al2618-T61
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.76 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 115AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 144Converted from Brinell Hardness Value
Hardness, Rockwell A 45.5Converted from Brinell Hardness Value
Hardness, Rockwell B 72Converted from Brinell Hardness Value
Hardness, Vickers 130Converted from Brinell Hardness Value
Tensile Strength, Ultimate 64.0 ksiAA; Typical
 34.0 MPa
@Temperature 371 °C
 52.0 MPa
@Temperature 316 °C
 90.0 MPa
@Temperature 260 °C
 221 MPa
@Temperature 204 °C
 345 MPa
@Temperature 149 °C
 427 MPa
@Temperature 100 °C
 441 MPa
@Temperature -28.0 °C
 441 MPa
@Temperature 24.0 °C
 462 MPa
@Temperature -80.0 °C
 538 MPa
@Temperature -196 °C
 350 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Short transverse
 360 MPa
@Thickness <=50.8 mm
Hand forgings; Short transverse
 360 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Short transverse
 365 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Long transverse
 380 MPa
@Thickness <=102 mm
Die forgings; Axis not parallel to grain flow
 380 MPa
@Thickness <=50.8 mm
Hand forgings; Long transverse
 380 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Long transverse
 380 MPa
@Thickness <=63.5 mm
Rolled rings; Tangential
 380 MPa
@Thickness <=63.5 mm
Rolled rings; Axial
 385 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Longitudinal
 395 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Longitudinal
 400 MPa
@Thickness <=102 mm
Die forgings; Axis parallel to grain flow
 400 MPa
@Thickness <=50.8 mm
Hand forgings; Longitudinal
Tensile Strength, Yield 54.0 ksiAA; Typical
 270 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Short transverse
 275 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Long transverse
 285 MPa
@Thickness <=63.5 mm
Rolled rings; Tangential
 285 MPa
@Thickness <=63.5 mm
Rolled rings; Axial
 290 MPa
@Thickness <=102 mm
Die forgings; Axis not parallel to grain flow
 290 MPa
@Thickness <=50.8 mm
Hand forgings; Long transverse
 290 MPa
@Thickness <=50.8 mm
Hand forgings; Short transverse
 290 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Long transverse
 290 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Short transverse
 310 MPa
@Thickness <=102 mm
Die forgings; Axis parallel to grain flow
 310 MPa
@Thickness 76.23 - 102 mm
Hand forgings; Longitudinal
 315 MPa
@Thickness 50.83 - 76.2 mm
Hand forgings; Longitudinal
 325 MPa
@Thickness <=50.8 mm
Hand forgings; Longitudinal
 24.0 MPa
@Strain 0.2 %,
Temperature 371 °C
 31.0 MPa
@Strain 0.2 %,
Temperature 316 °C
 62.0 MPa
@Strain 0.2 %,
Temperature 260 °C
 179 MPa
@Strain 0.2 %,
Temperature 204 °C
 303 MPa
@Strain 0.2 %,
Temperature 149 °C
 372 MPa
@Strain 0.2 %,
Temperature -28.0 °C
 372 MPa
@Strain 0.2 %,
Temperature 24.0 °C
 372 MPa
@Strain 0.2 %,
Temperature 100 °C
 379 MPa
@Strain 0.2 %,
Temperature -80.0 °C
 421 MPa
@Strain 0.2 %,
Temperature -196 °C
Elongation at Break 10 %
@Temperature -28.0 °C
 10 %
@Temperature 24.0 °C
 10 %
@Temperature 100 °C
 11 %
@Temperature -80.0 °C
 12 %
@Temperature -196 °C
 14 %
@Temperature 149 °C
 24 %
@Temperature 204 °C
 50 %
@Temperature 260 °C
 80 %
@Temperature 316 °C
 120 %
@Temperature 371 °C
 4.0 %
@Thickness <=102 mm
Die forgings; Axis parallel to grain flow
 4.0 %
@Thickness <=102 mm
Die forgings; Axis not parallel to grain flow
 4.0 %
@Thickness <=50.8 mm
Hand forgings; Short transverse
 4.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; Short transverse
 4.0 %
@Thickness 76.23 - 102 mm
Hand forgings; Short transverse
 5.0 %
@Thickness <=50.8 mm
Hand forgings; Long transverse
 5.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; Long transverse
 5.0 %
@Thickness 76.23 - 102 mm
Hand forgings; Long transverse
 5.0 %
@Thickness <=63.5 mm
Rolled rings; Axial
 6.0 %
@Thickness <=63.5 mm
Rolled rings; Tangential
 7.0 %
@Thickness <=50.8 mm
Hand forgings; Longitudinal
 7.0 %
@Thickness 50.83 - 76.2 mm
Hand forgings; Longitudinal
 7.0 %
@Thickness 76.23 - 102 mm
Hand forgings; Longitudinal
 10 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10800 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Compressive Strength 370 MPa
Poissons Ratio 0.33
Fatigue Strength 18000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPaCalculated
Shear Strength 38.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000470 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.6 µm/m-°C
@Temperature -50.0 - 20.0 °C
 23.2 µm/m-°C
@Temperature 20.0 - 200 °C
 24.0 µm/m-°C
@Temperature 20.0 - 300 °C
average
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.875 J/g-°C
Thermal Conductivity 146 W/m-K
Melting Point 1020 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 1020 °FAA; Typical
Liquidus 1180 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Solution Temperature 985 °F
Aging Temperature 390 °Ffor 20 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 92.4 - 94.9 %As remainder
Copper, Cu 1.9 - 2.7 %
Iron, Fe 0.90 - 1.3 %
Magnesium, Mg 1.3 - 1.8 %
Nickel, Ni 0.90 - 1.2 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si 0.10 - 0.25 %
Titanium, Ti 0.04 - 0.10 %
Zinc, Zn <= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2618-T6
Aluminum 2618-T61 (Includes Creep/Rupture Data)
Aluminum 7075-T6; 7075-T651
Aluminum 6061-T6; 6061-T651
Alclad Aluminum 7075-T6, T651

MA2618T61 / 8971

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.