MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Zirconium Copper (Amzirc Brand Copper), UNS C15000, TH04 Temper
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Excellent hot and cold workability. Fabricated by swaging, bending, heading, or forging.

Applications: Stud bases for power transmitters and rectifiers, switches and circuit breakers for high-temperature service, commutators, resistance welding tips and wheels, solderless wrapped connectors.

Mechanical property data for TH04 Temper - 82% cold work.

Key Words: ISO CuZr, CEN CW120C, N-4 Alloy
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.89 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 72TB04 or TH04 temper
Tensile Strength, Ultimate 445 MPa
@Temperature 22.0 °C
 463 MPa
@Temperature -78.0 °C
 534 MPa
@Temperature -197 °C
 587 MPa
@Temperature -253 °C
 591 MPa
@Temperature -269 °C
Tensile Strength, Yield 385 MPa
 411 MPa
@Strain 0.2 %,
Temperature 22.0 °C
 423 MPa
@Strain 0.2 %,
Temperature -78.0 °C
 446 MPa
@Strain 0.2 %,
Temperature -269 °C
 453 MPa
@Strain 0.2 %,
Temperature -197 °C
 458 MPa
@Strain 0.2 %,
Temperature -253 °C
Elongation at Break 16 %
@Temperature 22.0 °C
 20 %
@Temperature -78.0 °C
 26 %
@Temperature -197 °C
 36 %
@Temperature -269 °C
 37 %
@Temperature -253 °C
Creep Strength 1.00 MPa
@Temperature 650 °C,
Time 3.60e+8 sec
1% creep
 1.50 MPa
@Temperature 600 °C,
Time 3.60e+8 sec
1% creep
 1.70 MPa
@Temperature 650 °C,
Time 3.60e+7 sec
1% creep
 2.80 MPa
@Temperature 600 °C,
Time 3.60e+7 sec
1% creep
 3.00 MPa
@Temperature 650 °C,
Time 3.60e+6 sec
1% creep
 5.20 MPa
@Temperature 600 °C,
Time 3.60e+6 sec
1% creep
 28.0 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
1% creep
 41.0 MPa
@Temperature 500 °C,
Time 3.60e+7 sec
1% creep
 44.0 MPa
@Temperature 450 °C,
Time 3.60e+8 sec
1% creep
 53.0 MPa
@Temperature 450 °C,
Time 3.60e+7 sec
1% creep
 63.0 MPa
@Temperature 500 °C,
Time 3.60e+6 sec
1% creep
 77.0 MPa
@Temperature 450 °C,
Time 3.60e+6 sec
1% creep
 139 MPa
@Temperature 400 °C,
Time 3.60e+8 sec
1% creep
 161 MPa
@Temperature 400 °C,
Time 3.60e+7 sec
1% creep
 201 MPa
@Temperature 400 °C,
Time 3.60e+6 sec
1% creep
 219 MPa
@Temperature 350 °C,
Time 3.60e+8 sec
1% creep
 238 MPa
@Temperature 350 °C,
Time 3.60e+7 sec
1% creep
 240 MPa
@Temperature 300 °C,
Time 3.60e+8 sec
1% creep
 257 MPa
@Temperature 350 °C,
Time 3.60e+6 sec
1% creep
 271 MPa
@Temperature 300 °C,
Time 3.60e+7 sec
1% creep
 303 MPa
@Temperature 250 °C,
Time 3.60e+8 sec
1% creep
 305 MPa
@Temperature 300 °C,
Time 3.60e+6 sec
1% creep
 312 MPa
@Temperature 250 °C,
Time 3.60e+7 sec
1% creep
 321 MPa
@Temperature 250 °C,
Time 3.60e+6 sec
1% creep
Modulus of Elasticity 129 GPa
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Charpy Impact 121 J
@Temperature 22.0 °C
V-notch, 10 mm square
 142 J
@Temperature -78.0 °C
V-notch, 10 mm square
 155 J
@Temperature -197 °C
V-notch, 10 mm square
 155 J
@Temperature -253 °C
V-notch, 10 mm square
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000186 ohm-cm
@Temperature 20.0 °C
solution treated, cold worked 84%, and aged material
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.9 µm/m-°C
@Temperature 20.0 - 100 °C
 17.6 µm/m-°C
@Temperature 20.0 - 200 °C
 20.2 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.385 J/g-°C
Thermal Conductivity 367 W/m-KSolution treated, cold worked 84%, and aged material
Melting Point 980 - 1080 °C
Solidus 980 °C
Liquidus 1080 °C
Annealing Point 1650 - 1740 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 600 - 700 °C
Hot-Working Temperature 900 - 950 °C
Precipitation Temperature >= 930 °F
@Time 7200 sec
Water
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 99.9 %
Zirconium, Zr 0.050 - 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Zirconium Copper (Amzirc Brand Copper), UNS C15000, TH01 Temper
Electrolytic Tough Pitch (ETP) Copper, UNS C11000, H04 Temper flat products
Zirconium Copper (Amzirc Brand Copper), UNS C15000, 19 mm rod
Oxygen-free extra-low phosphorus Copper, UNS C10300, H04 temper, flat products
Zirconium Copper (Amzirc Brand Copper), UNS C15000, 13 mm rod

MC15000d1 / 171639

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.