MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Drake Plastics PAI 4630 Extruded Polyamide-Imide
Categories: Polymer; Thermoplastic; Polyamide-imide (PAI); Polyamide-Imide, Glass Filled

Material Notes: Description: DRAKE 4630 PAI provides the maximum wear resistance in high speed, non-lubricate applications. It has been proven to perform in applications with PVs exceeding 150,000 psi-FPM.

Typical Applications:

  • Sliding vanes
  • Thrust washers
  • Piston seal rings
  • Bearings & bushings

Information provided by Drake Plastics.

Vendors: Drake Plastics Ltd. Co. The Torlon Specialist, manufactures & stocks the most complete line of Torlon PAI in machinable rod, plate & Seamless Tube®. Drake works closely with Solvay Specialty Polymers to identify & serve a multitude of new applications. Drake, a lean producer of extruded, injection molded & machined shapes & parts, offers low minimums & quick, economical delivery globally.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.56 g/ccASTM D792
Water Absorption 0.20 %
@Time 86400 sec
Immersion; ASTM D570(2)
Water Absorption at Saturation 1.5 %Immersion; ASTM D570(2)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell E 62ASTM D875
Hardness, Rockwell M 106ASTM D875
Hardness, Shore D 84ASTM D2240
Tensile Strength, Ultimate 83.0 MPaASTM D638
Elongation at Break 2.00 %ASTM D638
Tensile Modulus 5.52 GPaASTM D638
Flexural Yield Strength 105 MPaASTM D790
Flexural Modulus 5.52 GPaASTM D790
Compressive Strength 125 MPa10% Def; ASTM D695
Compressive Modulus 5.17 GPaASTM D695
Izod Impact, Notched 0.700 ft-lb/inType A; ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°CASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 278 °CASTM D648
Glass Temperature Coefficient 275ASTM D3418

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDRAKE80c / 326980

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.