MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Avient ECCOH™ 6600 Low Smoke Free Of Halogen (LSFOH)  (discontinued **)
Categories: Polymer; Thermoplastic

Material Notes:

ECC0H 6600 is a low smoke flame retardant zero halogen compound, designed to meet requirements of a number of international specifications for LSFOH cables, including IEC, BS, VDE, etc. This product is flexible with good flame retardancy and chemical resistance. The processing performance is excellent.

Description/Features:

  • Low Smoke Flame Retardant Zero Halogen Compound (LSFOH)

Applications:

  • Jacket

Market:

  • Wire & Cable
PolyOne First Choice

Disclaimer: NOTE: "Pass" on Vertical Burn Test is dependant on cable construction. "Pass" on Smoke Density pertains to test performed on test sheets.

Information provided by PolyOne Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
pH 4.34.3
Mooney Viscosity 44
@Temperature 140 °C
44
@Temperature 284 °F
ML (1 + 4); ISO 1769
Halogen Content 0.00 %0.00 %IEC 754-1
High Load Melt Index 2.7 g/10 min
@Load 21.6 kg,
Temperature 150 °C
2.7 g/10 min
@Load 47.6 lb,
Temperature 302 °F
ISO 1133, (b)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4444ISO R 868
Tensile Strength, Ultimate 12.00 MPa1740 psi240 hrs (10 days), 212°F(100°C); IEC 60811-1-2
Tensile Strength, Yield 11.00 MPa1595 psiIEC 60811-1-1
Elongation at Break 160 %160 %168 hrs (7 days), 212°F(100°C); IEC 60811-1-2
 180 %180 %IEC 60811-1-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 25000 ohm-cm25000 ohm-cm
Dielectric Constant 5.1
@Frequency 50 Hz
5.1
@Frequency 50 Hz
IEC 60520
Dissipation Factor 0.070
@Frequency 50 Hz
0.070
@Frequency 50 Hz
IEC 60520
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 285 °C545 °FFlammability Temperature Index; ISO 4589-2
Smoke Density  <= 38
@Thickness 1.00 mm
<= 38
@Thickness 0.0394 in
Flaming Mode, Ds Max; ASTM E-662
 <= 59
@Thickness 1.00 mm
<= 59
@Thickness 0.0394 in
Non-Flaming Mode, Ds Max; ASTM E-662
Oxygen Index 35 %35 %Limited; ISO 4589-2
 
Descriptive Properties
AppearancePelletsASTM D2090
Cold Impact @ -25°CPassIEC 60811-1-4
Heat Shock, 1 hr @ 150° CPassIEC 60811-3-1
Hot Pressure Test30%4 hrs @ 80ºC, IEC 860811-3-1
Immersion- Elo. variation from Orig.10%IRM 902 OIL, 4 hrs @ 70ºC, IEC 60811-2-1
Immersion- TS variation from Orig.3%IRM 902 OIL, 4 hrs @ 70ºC, IEC 60811-2-1
Smoke DensityPassIEC 61034
Toxicity1NES 713
Vertical Burn TestPassIEC 60332-3
Water Absorption0.00081oz/in²240 hrs (10 days), 158°F(70°C), IEC 60811-1-3

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Avient ECCOH™ 6150 Low Smoke Free Of Halogen (LSFOH)
Avient ECCOH™ 6200 Low Smoke Free Of Halogen (LSFOH)
Avient ECCOH™ 6000 Low Smoke Free Of Halogen (LSFOH)
AlphaGary Evoprene™ LF 6151 Automotive Thermoplastic Elastomer

PH1PO0064 / 43355

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.