MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Momentive Performance Materials RTV142 White, Low Volatile, One Component Silicone Sealant
Categories: Polymer; Adhesive; Thermoset; Silicone; Silicone, RTV, Adhesive/Sealant Grade

Material Notes: RTV 142 one-component, ready-to-use adhesive sealant cures to a tough, durable, resilient silicone rubber on exposure to atmospheric moisture at room temperature. Methyl alcohol vapors are released from the sealant surface as a by-product of cure. These vapors have low odor and are non-corrosive to metals. An important property of RTV142 is its low volatility.

RTV 142 sealant has a thixotropic paste-like consistency. This allows it to be applied to vertical and overhead surfaces without sagging. Since it utilizes a moisture cure system, RTV142 sealant should not be used in thicknesses of greater than 6mm(1/4 in.). When section depths exceed 6mm(1/4in.), GE Silicones one-component, addition cure or two-component silicone rubber compounds are suggested.

Mechanical properties for specimen cured 10 days at 25°C and 50% relative humidity.

Key Performance Properties:

  • One component product
  • Room temperature cure
  • Primerless adhesion to many substrates
  • Low odor
  • Non-corrosive to metals
  • Low volatility
  • Low temperature flexibility
  • High temperature performance
  • Excellent weatherability and ozone and chemical resistance
  • Excellent electrical insulation properties
  • Non-halogen flame retardant

Applications:

The non-corrosiveness to metals and low volatility of RTV142, as well as its paste consistency, make it well suited for critical electronic adhesive, gasketing, and sealing applications where a high level of volatile condensable materials cannot be tolerated.

GE Silicones became a part of Momentive Performance Materials in 2006.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.09 g/cc
Linear Mold Shrinkage <= 0.010 cm/cm
Collected Volatile Condensable Material 0.050 %Ball aerospace VCM test 33074
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 34
Tensile Strength, Ultimate 38.5 kg(f)/cm²
Elongation at Break 400 %
Adhesive Bond Strength 2.0594 MPaAt 100% cohesive failure
Tear Strength 9.00 kg(f)/cm
Peel Strength 60.0 pliAt 100% cohesive failure using 1 in. x 8 in. stainless steel screen at 180° pull angle
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 4.50e+15 ohm-cm
Dielectric Constant 2.8
@Frequency 60 Hz
Dielectric Strength 20.0 kV/mm
Dissipation Factor 0.0010
@Frequency 60 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 270 µm/m-°C
@Temperature 20.0 °C
Thermal Conductivity 0.210 W/m-K
Maximum Service Temperature, Air 204 °CContinuous
Minimum Service Temperature, Air -60.0 °CContinuous
 
Processing PropertiesOriginal ValueComments
Tack-Free Time 4 hour
 
Descriptive Properties
% Total Weight Loss0.0022Ball aerospace VCM test 33074
Application rate975 g/min
ColorWhite
ConsistencyPaste

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Henkel Loctite® Durabond® E-30CL Epoxy Adhesive
3M Scotch-Weld™ 2216 B/A Gray Epoxy Adhesive
Dow 732 MULTI-PURPOSE SEALANT
Momentive Performance Materials RTV112 One Component Acetoxy Adhesive Sealant, White
Aluminum 2024-T6

PGESIL019 / 41010

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.