MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  
Elmet Technologies
Assab Steels 709M Machinery Steel
Categories: Metal; Ferrous Metal; Alloy Steel

Material Notes: ASSAB 709M is an alloyed machinery steel with high strength in small and medium sizes. As standard ASSAB 705M is supplied tough hardened requiring no further heat treatment. It can be oil hardened to higher mechanical properties.

Applications: ASSAB 709M is suitable for flame and induction hardening. It can also be nitrided or tuffrided to a surface hardness of 600-650 Vickers.

ASSAB 709M is not suitable for welding but can with certain precautions be repair welded.

Typical applications include shafts and other power transmission components as well as high strength bolts.

AISI /SAE 4140, DIN 42CrMo4, W.nr. 1.7225, BS 708M42, AFNOR 42CD4, JIS SCM4, SS 2244

Vendors:
Available Properties
  • Hardness, Brinell, 700°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Hardness, Brinell, 500°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Hardness, Brinell, un-machined
  • Hardness, Brinell, un-machined
  • Hardness, Rockwell C, tempering temperature 500°C. Hardened by oil quenching.
  • Hardness, Rockwell C, 30 mm from the quenched end.
  • Hardness, Rockwell C, 10 mm from the quenched end.
  • Hardness, Rockwell C, tempering temperature 200°C. Hardened by oil quenching.
  • Tensile Strength at Break, Rm. 700°C tempering temperature. Quenching in oil ø 50. Testpiece hardened by oil quenching from 850°C.
  • Tensile Strength at Break, Rm. 500°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Tensile Strength, Ultimate, Rm., un-machined
  • Tensile Strength, Ultimate, Rm., unmachined
  • Tensile Strength, Yield, Re. 700°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Tensile Strength, Yield, Re. 500°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Tensile Strength, Yield, Re., un-machined
  • Tensile Strength, Yield, Re. , un-machined
  • Elongation at Break, 5XD. 500°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Elongation at Break, 5XD. 700°C tempering temperature. Quenching in oil ø 120. Test piece hardened by oil quenching from 850°C.
  • Elongation at Break, un-machined
  • Elongation at Break, un-machined
  • Reduction of Area, 500°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Reduction of Area, 700°C tempering temperature. Quenching in oil ø 50. Test piece hardened by oil quenching from 850°C.
  • Reduction of Area, un-machined
  • Reduction of Area, un-machined
  • Impact Test, un-machined
  • Carbon, C
  • Chromium, Cr
  • Iron, Fe
  • Manganese, Mn
  • Molybdenum, Mo
  • Silicon, Si
  
Property Data

This page displays only the text
of a material data sheet.

To see MatWeb's complete data
sheet for this material (including
material property data, metal
compositions, material suppliers,
etc
), please click the button below.

Manufacturer Notes:
none

Category Notes
none

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

 

New MatWeb Services
Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.