MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales
metalmen Is Your Direct to US Manufacturing Source for High Purity Metals

Tin, Sn
Categories: Metal; Nonferrous Metal; Tin Alloy; Other Engineering Material; Semiconductor; Pure Element

Material Notes: White (Beta) tin, stable above 13.2°C, is the common metallic form of the element. Alpha-tin is a semiconductor.

Characteristics: Susceptible to creep deformation at room temperature, Highly susceptible to corrosion in strong acidic and strong alkaline environments

Typical Applications: Tinplate foil, collapsible tubes, block tin products, pewter, alloying, coatings, powder applications (sintered bronze and iron parts).

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 5.765 g/cc0.2083 lb/in³Alpha-Tin
 6.45 g/cc0.233 lb/in³Gamma
 7.29 g/cc0.263 lb/in³Value is for the beta crystal structure, stable between 18-161 C.
Viscosity  0.87 cP
@Temperature 800 °C
0.87 cP
@Temperature 1470 °F
Dynamic liquid viscosity
 0.95 cP
@Temperature 700 °C
0.95 cP
@Temperature 1290 °F
Dynamic liquid viscosity
 1.05 cP
@Temperature 600 °C
1.05 cP
@Temperature 1110 °F
Dynamic liquid viscosity
 1.18 cP
@Temperature 500 °C
1.18 cP
@Temperature 932 °F
Dynamic liquid viscosity
 1.38 cP
@Temperature 400 °C
1.38 cP
@Temperature 752 °F
Dynamic liquid viscosity
 1.66 cP
@Temperature 300 °C
1.66 cP
@Temperature 572 °F
Dynamic liquid viscosity
 1.88 cP
@Temperature 250 °C
1.88 cP
@Temperature 482 °F
Dynamic liquid viscosity
 2.71 cP
@Temperature 232 °C
2.71 cP
@Temperature 450 °F
Dynamic liquid viscosity
 42300 cP
@Temperature 260 °C
42300 cP
@Temperature 500 °F
a Lattice Constant 6.4912 Å6.4912 ÅAlpha-Tin
Vapor Pressure  0.00000160 bar
@Temperature 927 °C
0.00120 torr
@Temperature 1700 °F
 0.0000110 bar
@Temperature 1027 °C
0.00825 torr
@Temperature 1881 °F
 0.0000590 bar
@Temperature 1127 °C
0.0443 torr
@Temperature 2061 °F
 0.000230 bar
@Temperature 1227 °C
0.173 torr
@Temperature 2241 °F
 0.000890 bar
@Temperature 1327 °C
0.668 torr
@Temperature 2421 °F
 0.00746 bar
@Temperature 1527 °C
5.60 torr
@Temperature 2781 °F
 0.0408 bar
@Temperature 1727 °C
30.6 torr
@Temperature 3141 °F
 0.0841 bar
@Temperature 1827 °C
63.1 torr
@Temperature 3321 °F
 0.290 bar
@Temperature 2027 °C
218 torr
@Temperature 3681 °F
 0.513 bar
@Temperature 2127 °C
385 torr
@Temperature 3861 °F
 0.851 bar
@Temperature 2227 °C
638 torr
@Temperature 4041 °F
 0.990 bar
@Temperature 727 °C
743 torr
@Temperature 1340 °F
Surface Tension 548 dynes/cm
@Temperature 260 °C
548 dynes/cm
@Temperature 500 °F
 
Chemical PropertiesMetricEnglishComments
Atomic Mass 118.710118.7101995
Atomic Number 5050
Thermal Neutron Cross Section 0.65 barns/atom0.65 barns/atom
X-ray Absorption Edge 0.42468 Å0.42468 ÅK
 2.78875 Å2.78875 ÅLI
 2.99492 Å2.99492 ÅLII
 3.16952 Å3.16952 ÅLIII
Electrode Potential -0.140 V-0.140 V
Electronegativity 1.961.96Pauling
Ionic Radius 0.710 Å0.710 ÅCrystal Ionic Radius for Valence +4
 0.930 Å0.930 ÅCrystal Ionic Radius for Valence +2
 2.94 Å2.94 ÅCrystal Ionic Radius for Valence -4
 3.70 Å3.70 ÅCrystal Ionic Radius for Valence -1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  2.3
@Temperature 100 °C
2.3
@Temperature 212 °F
 3.0
@Temperature 60.0 °C
3.0
@Temperature 140 °F
 3.9
@Temperature 20.0 °C
3.9
@Temperature 68.0 °F
Tensile Strength, Ultimate 220 MPa31900 psi
Tensile Strength, Yield  4.50 MPa
@Temperature 200 °C
653 psi
@Temperature 392 °F
Strained at 0.4 mm/m*min
 7.60 MPa
@Temperature 150 °C
1100 psi
@Temperature 302 °F
Strained at 0.4 mm/m*min
 11.0 MPa
@Temperature 100 °C
1600 psi
@Temperature 212 °F
Strained at 0.4 mm/m*min
 11.0 MPa
@Temperature 23.0 °C
1600 psi
@Temperature 73.4 °F
Strained at 0.2 mm/m*min
 12.4 MPa
@Temperature 50.0 °C
1800 psi
@Temperature 122 °F
Strained at 0.4 mm/m*min
 12.5 MPa
@Temperature 0.000 °C
1810 psi
@Temperature 32.0 °F
Strained at 0.2 mm/m*min
 14.5 MPa
@Temperature 15.0 °C
2100 psi
@Temperature 59.0 °F
Strained at 0.4 mm/m*min
 20.1 MPa
@Temperature -40.0 °C
2920 psi
@Temperature -40.0 °F
Strained at 0.2 mm/m*min
 36.2 MPa
@Temperature -200 °C
5250 psi
@Temperature -328 °F
Strained at 0.2 mm/m*min
 38.9 MPa
@Temperature -80.0 °C
5640 psi
@Temperature -112 °F
Strained at 0.2 mm/m*min
 87.6 MPa
@Temperature -120 °C
12700 psi
@Temperature -184 °F
Strained at 0.2 mm/m*min
 90.3 MPa
@Temperature -160 °C
13100 psi
@Temperature -256 °F
Strained at 0.2 mm/m*min
Elongation at Yield  6.0 %
@Temperature -200 °C
6.0 %
@Temperature -328 °F
Strained at 0.2 mm/m*min; Reduction in area: 6%
 15 %
@Temperature -160 °C
15 %
@Temperature -256 °F
Strained at 0.2 mm/m*min; Reduction in area: 10%
 45 %
@Temperature 200 °C
45 %
@Temperature 392 °F
Strained at 0.4 mm/m*min
 55 %
@Temperature 100 °C
55 %
@Temperature 212 °F
Strained at 0.4 mm/m*min
 55 %
@Temperature 150 °C
55 %
@Temperature 302 °F
Strained at 0.4 mm/m*min
 57 %
@Temperature 23.0 °C
57 %
@Temperature 73.4 °F
Strained at 0.2 mm/m*min; Reduction in area: 100%
 60 %
@Temperature -120 °C
60 %
@Temperature -184 °F
Strained at 0.2 mm/m*min; Reduction in area: 97%
 64 %
@Temperature 0.000 °C
64 %
@Temperature 32.0 °F
Strained at 0.2 mm/m*min; Reduction in area: 100%
 75 %
@Temperature 15.0 °C
75 %
@Temperature 59.0 °F
Strained at 0.4 mm/m*min
 85 %
@Temperature 50.0 °C
85 %
@Temperature 122 °F
Strained at 0.4 mm/m*min
 86 %
@Temperature -40.0 °C
86 %
@Temperature -40.0 °F
Strained at 0.2 mm/m*min; Reduction in area: 100%
 89 %
@Temperature -80.0 °C
89 %
@Temperature -112 °F
Strained at 0.2 mm/m*min; Reduction in area: 100%
Modulus of Elasticity 41.6 GPa6030 ksiCast (coarse grain)
 44.3 GPa6430 ksiSelf-annealed (fine grain)
Poissons Ratio 0.330.33
Shear Modulus 15.6 GPa2260 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000115 ohm-cm0.0000115 ohm-cm
 0.0000110 ohm-cm
@Temperature 0.000 °C
0.0000110 ohm-cm
@Temperature 32.0 °F
 0.0000155 ohm-cm
@Temperature 100 °C
0.0000155 ohm-cm
@Temperature 212 °F
 0.0000200 ohm-cm
@Temperature 200 °C
0.0000200 ohm-cm
@Temperature 392 °F
 0.0000220 ohm-cm
@Temperature 231 °C
0.0000220 ohm-cm
@Temperature 448 °F
 0.0000450 ohm-cm
@Temperature 232 °C
0.0000450 ohm-cm
@Temperature 450 °F
liquid
 0.0000468 ohm-cm
@Temperature 300 °C
0.0000468 ohm-cm
@Temperature 572 °F
liquid
 0.0000490 ohm-cm
@Temperature 400 °C
0.0000490 ohm-cm
@Temperature 752 °F
liquid
 0.0000515 ohm-cm
@Temperature 500 °C
0.0000515 ohm-cm
@Temperature 932 °F
liquid
 0.0000540 ohm-cm
@Temperature 600 °C
0.0000540 ohm-cm
@Temperature 1110 °F
liquid
 0.0000563 ohm-cm
@Temperature 700 °C
0.0000563 ohm-cm
@Temperature 1290 °F
liquid
 0.0000587 ohm-cm
@Temperature 800 °C
0.0000587 ohm-cm
@Temperature 1470 °F
liquid
 0.0000612 ohm-cm
@Temperature 900 °C
0.0000612 ohm-cm
@Temperature 1650 °F
liquid
Magnetic Susceptibility -2.50e-7-2.50e-7cgs/g
Critical Magnetic Field Strength, Oersted 305305
Critical Superconducting Temperature  4.85 - 5.20 K
@Pressure 12500 - 16000 MPa
4.85 - 5.20 K
@Pressure 1.81e+6 - 2.32e+6 psi
Sn II
 5.30 K
@Pressure 11300 MPa
5.30 K
@Pressure 1.64e+6 psi
Sn III
Dielectric Constant 2424Alpha-Tin
Band Gap 0.080 eV0.080 eVAlpha-Tin
Electron Mobility, cm²/V-s 25002500Alpha-Tin
Hole Mobility, cm²/V-s 24002400Alpha-Tin
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 59.5 J/g25.6 BTU/lb
Heat of Vaporization 2399 J/g1032 BTU/lb
CTE, linear  5.40 µm/m-°C
@Temperature -50.0 °C
3.00 µin/in-°F
@Temperature -58.0 °F
Alpha-Tin
 23.8 µm/m-°C
@Temperature 20.0 - 100 °C
13.2 µin/in-°F
@Temperature 68.0 - 212 °F
 30.0 µm/m-°C
@Temperature 200 °C
16.7 µin/in-°F
@Temperature 392 °F
 40.4 µm/m-°C
@Temperature 200 °C
22.4 µin/in-°F
@Temperature 392 °F
CTE, linear, Transverse to Flow 19.9 µm/m-°C
@Temperature 200 °C
11.1 µin/in-°F
@Temperature 392 °F
Specific Heat Capacity 0.213 J/g-°C0.0509 BTU/lb-°FAlpha-Tin
 0.256 J/g-°C0.0612 BTU/lb-°FBeta-Tin
Thermal Conductivity 63.2 W/m-K439 BTU-in/hr-ft²-°F
 32.6 W/m-K
@Temperature 232 - 332 °C
226 BTU-in/hr-ft²-°F
@Temperature 450 - 630 °F
liquid
 56.5 W/m-K
@Temperature 200 °C
392 BTU-in/hr-ft²-°F
@Temperature 392 °F
beta phase
 60.7 W/m-K
@Temperature 100 °C
421 BTU-in/hr-ft²-°F
@Temperature 212 °F
beta phase
 62.8 W/m-K
@Temperature 0.000 °C
436 BTU-in/hr-ft²-°F
@Temperature 32.0 °F
beta phase
 80.8 W/m-K
@Temperature -170 °C
561 BTU-in/hr-ft²-°F
@Temperature -274 °F
beta phase
Melting Point 231.968 °C449.543 °F
Boiling Point 2602 °C4716 °F
Heat of Formation -2.10 kJ/mol-2.10 kJ/molGrey (Alpha) Tin
 0.000 kJ/mol0.000 kJ/molWhite (Beta)-Tin
Debye Temperature -43.0 °C-45.4 °FAlpha-Tin
 
Optical PropertiesMetricEnglishComments
Refractive Index 2.75
@Wavelength 589.3 nm
2.75
@Wavelength 589.3 nm
Alpha-Tin
Emissivity (0-1) 0.040
@Temperature 50.0 °C
0.040
@Temperature 122 °F
Reflection Coefficient, Visible (0-1) 0.800.80Bulk Solid
 
Component Elements PropertiesMetricEnglishComments
Tin, Sn 100 %100 %
 
Descriptive Properties
CAS Number7440-31-5
Crystal StructureCubicAlpha-Tin; Diamond Structure - Space Group Fd3m

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Tin, Sn (Gray)
Tin, Sn (White)
Lead, Pb
Silver, Ag
Copper, Cu; Annealed

AMESn00 / 104

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.