MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ALM Ultrasint® PA6 MF Nylon 6, Mineral Reinforced, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Mineral Filled

Material Notes: Ultrasint PA6 MF is the material of choice for advanced technical applications where properties of mechanically reinforced thermoplastics are needed.

Highlights:

  • Mineral-filled Polyamide 6-based powder for Laser Sintering
Applications:
  • Engine compartment parts
  • Piping & Media flow/storage parts
  • Housings & covers
  • Tooling equipment & molds

Information provided by Advanced Laser Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.600 g/cc0.0217 lb/in³DIN EN ISO 60
Density 1.44 g/cc0.0520 lb/in³Printed Part; DIN EN ISO 1181-1
Particle Size 65 - 75 µm65 - 75 µmD50
Melt Flow 10.08 g/10 min
@Load 2.16 kg,
Temperature 240 °C
10.08 g/10 min
@Load 4.76 lb,
Temperature 464 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 50.0 MPa7250 psiZ-Direction; ISO 527-2
 91.0 MPa13200 psiX-Direction; ISO 527-2
Elongation at Break 0.90 %0.90 %Z-Direction; ISO 527-2
 2.1 %2.1 %X-Direction; ISO 527-2
Tensile Modulus 5.90 GPa856 ksiZ-Direction; ISO 527-2
 6.25 GPa906 ksiX-Direction; ISO 527-2
Flexural Modulus 5.40 GPa783 ksiZ-Direction; DIN EN ISO 178
 6.00 GPa870 ksiX-Direction; DIN EN ISO 178
Izod Impact, Notched (ISO) 2.80 kJ/m²1.33 ft-lb/in²Z-Direction; ISO 180
 4.20 kJ/m²2.00 ft-lb/in²X-Direction; ISO 180
Izod Impact, Unnotched (ISO) 5.10 kJ/m²2.43 ft-lb/in²Z-Direction; ISO 180
 13.1 kJ/m²6.23 ft-lb/in²X-Direction; ISO 180
Charpy Impact Unnotched 0.460 J/cm²2.19 ft-lb/in²Z-Direction; ISO 179-1
 1.32 J/cm²6.28 ft-lb/in²X-Direction; ISO 179-1
Charpy Impact, Notched 0.190 J/cm²0.904 ft-lb/in²Z-Direction; ISO 179-1
 0.270 J/cm²1.28 ft-lb/in²X-Direction; ISO 179-1
 
Thermal PropertiesMetricEnglishComments
Melting Point 219 °C426 °FISO 11357
Crystallization Temperature 174 °C345 °FISO 11357
Deflection Temperature at 0.46 MPa (66 psi) 209 °C408 °FISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 121 °C250 °FISO 75-2
Vicat Softening Point  210 °C
@Load 5.10 kg
410 °F
@Load 11.2 lb
B; ISO 306
 217 °C
@Load 1.02 kg
423 °F
@Load 2.25 lb
A; ISO 306

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PALP9021 / 312356

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.