MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

A. Schulman Lucent PC/ABS-1211P Polycarbonate+ABS, Impact Modified, Platable, Injection Grade
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: Add "R" for Added Release
Add "U" for UV Stabilizer

Information provided by Lucent Polymers, Inc. Lucent was acquired by A. Schulman in 2015.

Key Words: PC, ABS
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.10 g/cc1.10 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0060 cm/cm
@Thickness 3.17 mm
0.0060 in/in
@Thickness 0.125 in
1/8" Section
Melt Flow 11 g/10 min
@Load 5.00 kg,
Temperature 260 °C
11 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 51.03 MPa7401 psiASTM D638
Elongation at Break >= 140 %>= 140 %ASTM D638
Flexural Strength 68.97 MPa10000 psiASTM D790
Flexural Modulus 2.069 GPa300.1 ksiASTM D790
Izod Impact, Notched  3.20 J/cm
@Thickness 3.17 mm,
Temperature -30.0 °C
6.00 ft-lb/in
@Thickness 0.125 in,
Temperature -22.0 °F
ASTM D256
 6.41 J/cm
@Thickness 3.17 mm,
Temperature 22.8 °C
12.0 ft-lb/in
@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 98.89 °C210.0 °FASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman Lucent PC/ABS-FR0 Polycarbonate+ABS, Flame Resistant
Covestro Bayblend® FR3001 PC/ABS Blend
Covestro Bayblend® 2953 Polycarbonate + ABS Blend, Automotive Plating
Lotte Advanced Materials Infino® HI-1001BG PC/ABS, Metal Plating Grade
Lotte Advanced Materials Infino® HI-1001BP PC/ABS, Metal Plating Grade

PLUCE038 / 89957

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.