MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum 2219-T851 (Extended High Temperature Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
This designation is considered the sole original alloy for this alloy family.
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T851; AA2219-T851
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.84 g/cc0.103 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 130130500 kg load with 10 mm ball
Hardness, Knoop 163163Converted from Brinell Hardness Value
Hardness, Rockwell A 49.549.5Converted from Brinell Hardness Value
Hardness, Rockwell B 8080Converted from Brinell Hardness Value
Hardness, Vickers 149149Converted from Brinell Hardness Value
Tensile Strength, Ultimate >= 400 MPa>= 58000 psiWire, rod, bar, and shapes (extruded); T8510, T8511
 >= 400 MPa>= 58000 psiExtruded tube; T8510, T8511
 455 MPa66000 psiAA; Typical
 30.0 MPa
@Temperature 371 °C
4350 psi
@Temperature 700 °F
 48.0 MPa
@Temperature 316 °C
6960 psi
@Temperature 601 °F
 200 MPa
@Temperature 260 °C
29000 psi
@Temperature 500 °F
 248 MPa
@Temperature 204 °C
36000 psi
@Temperature 399 °F
 338 MPa
@Temperature 149 °C
49000 psi
@Temperature 300 °F
 414 MPa
@Temperature 100 °C
60000 psi
@Temperature 212 °F
 455 MPa
@Temperature 24.0 °C
66000 psi
@Temperature 75.2 °F
 476 MPa
@Temperature -28.0 °C
69000 psi
@Temperature -18.4 °F
 490 MPa
@Temperature -80.0 °C
71100 psi
@Temperature -112 °F
 572 MPa
@Temperature -196 °C
83000 psi
@Temperature -321 °F
 >= 395 MPa
@Thickness 127.0 - 152 mm
>= 57300 psi
@Thickness 5.001 - 6.00 in
Plate
 >= 405 MPa
@Thickness 101.6 - 127 mm
>= 58700 psi
@Thickness 4.001 - 5.00 in
Plate
 >= 415 MPa
@Thickness 76.23 - 102 mm
>= 60200 psi
@Thickness 3.001 - 4.00 in
Plate
 >= 425 MPa
@Thickness 6.35 - 50.8 mm
>= 61600 psi
@Thickness 0.250 - 2.00 in
Plate
 >= 425 MPa
@Thickness 50.83 - 76.2 mm
>= 61600 psi
@Thickness 2.001 - 3.00 in
Plate
 >= 395 MPa
@Diameter 50.83 - 102 mm
>= 57300 psi
@Diameter 2.001 - 4.00 in
Wire, rod, and bar (rolled or cold finished)
 >= 400 MPa
@Diameter 12.7 - 50.8 mm
>= 58000 psi
@Diameter 0.500 - 2.00 in
Wire, rod, and bar (rolled or cold finished)
Tensile Strength, Yield >= 290 MPa>= 42100 psiWire, rod, bar, and shapes (extruded); T8510, T8511
 >= 290 MPa>= 42100 psiExtruded tube; T8510, T8511
 352 MPa51000 psiAA; Typical
 >= 290 MPa
@Thickness 127.0 - 152 mm
>= 42100 psi
@Thickness 5.001 - 6.00 in
Plate
 >= 295 MPa
@Thickness 101.6 - 127 mm
>= 42800 psi
@Thickness 4.001 - 5.00 in
Plate
 >= 305 MPa
@Thickness 76.23 - 102 mm
>= 44200 psi
@Thickness 3.001 - 4.00 in
Plate
 >= 310 MPa
@Thickness 50.83 - 76.2 mm
>= 45000 psi
@Thickness 2.001 - 3.00 in
Plate
 >= 315 MPa
@Thickness 6.35 - 50.8 mm
>= 45700 psi
@Thickness 0.250 - 2.00 in
Plate
 >= 270 MPa
@Diameter 50.83 - 102 mm
>= 39200 psi
@Diameter 2.001 - 4.00 in
Wire, rod, and bar (rolled or cold finished)
 >= 275 MPa
@Diameter 12.7 - 50.8 mm
>= 39900 psi
@Diameter 0.500 - 2.00 in
Wire, rod, and bar (rolled or cold finished)
 26.0 MPa
@Strain 0.2 %,
Temperature 371 °C
3770 psi
@Strain 0.2 %,
Temperature 700 °F
 41.0 MPa
@Strain 0.2 %,
Temperature 316 °C
5950 psi
@Strain 0.2 %,
Temperature 601 °F
 159 MPa
@Strain 0.2 %,
Temperature 260 °C
23100 psi
@Strain 0.2 %,
Temperature 500 °F
 200 MPa
@Strain 0.2 %,
Temperature 204 °C
29000 psi
@Strain 0.2 %,
Temperature 399 °F
 276 MPa
@Strain 0.2 %,
Temperature 149 °C
40000 psi
@Strain 0.2 %,
Temperature 300 °F
 324 MPa
@Strain 0.2 %,
Temperature 100 °C
47000 psi
@Strain 0.2 %,
Temperature 212 °F
 345 MPa
@Strain 0.2 %,
Temperature 24.0 °C
50000 psi
@Strain 0.2 %,
Temperature 75.2 °F
 359 MPa
@Strain 0.2 %,
Temperature -28.0 °C
52100 psi
@Strain 0.2 %,
Temperature -18.4 °F
 372 MPa
@Strain 0.2 %,
Temperature -80.0 °C
54000 psi
@Strain 0.2 %,
Temperature -112 °F
 421 MPa
@Strain 0.2 %,
Temperature -196 °C
61100 psi
@Strain 0.2 %,
Temperature -321 °F
Elongation at Break 6.0 %6.0 %Wire, rod, bar, and shapes (extruded); T8510, T8511
 6.0 %6.0 %Extruded tube; T8510, T8511
 12 %
@Temperature -28.0 °C
12 %
@Temperature -18.4 °F
 12 %
@Temperature 24.0 °C
12 %
@Temperature 75.2 °F
 13 %
@Temperature -80.0 °C
13 %
@Temperature -112 °F
 15 %
@Temperature -196 °C
15 %
@Temperature -321 °F
 15 %
@Temperature 100 °C
15 %
@Temperature 212 °F
 17 %
@Temperature 149 °C
17 %
@Temperature 300 °F
 20 %
@Temperature 204 °C
20 %
@Temperature 399 °F
 21 %
@Temperature 260 °C
21 %
@Temperature 500 °F
 55 %
@Temperature 316 °C
55 %
@Temperature 601 °F
 75 %
@Temperature 371 °C
75 %
@Temperature 700 °F
 4.0 %
@Thickness 127.0 - 152 mm
4.0 %
@Thickness 5.001 - 6.00 in
Plate
 5.0 %
@Thickness 76.23 - 102 mm
5.0 %
@Thickness 3.001 - 4.00 in
Plate
 5.0 %
@Thickness 101.6 - 127 mm
5.0 %
@Thickness 4.001 - 5.00 in
Plate
 6.0 %
@Thickness 50.83 - 76.2 mm
6.0 %
@Thickness 2.001 - 3.00 in
Plate
 7.0 - 8.0 %
@Thickness 6.35 - 50.8 mm
7.0 - 8.0 %
@Thickness 0.250 - 2.00 in
Plate
 10 %
@Thickness 1.59 mm
10 %
@Thickness 0.0625 in
AA; Typical
 4.0 %
@Diameter 12.7 - 50.8 mm
4.0 %
@Diameter 0.500 - 2.00 in
Wire, rod, and bar (rolled or cold finished)
 4.0 %
@Diameter 50.83 - 102 mm
4.0 %
@Diameter 2.001 - 4.00 in
Wire, rod, and bar (rolled or cold finished)
Creep Strength  11.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1600 psi
@Temperature 698 °F,
Time 1000 hour
0.5% creep
 13.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1890 psi
@Temperature 698 °F,
Time 1000 hour
1% creep
 13.0 MPa
@Temperature 370 °C,
Time 360000 sec
1890 psi
@Temperature 698 °F,
Time 100 hour
0.2% creep
 18.0 MPa
@Temperature 370 °C,
Time 360000 sec
2610 psi
@Temperature 698 °F,
Time 100 hour
0.5% creep
 18.0 MPa
@Temperature 370 °C,
Time 36000 sec
2610 psi
@Temperature 698 °F,
Time 10.0 hour
0.1% creep
 20.0 MPa
@Temperature 370 °C,
Time 360000 sec
2900 psi
@Temperature 698 °F,
Time 100 hour
1% creep
 23.0 MPa
@Temperature 370 °C,
Time 36000 sec
3340 psi
@Temperature 698 °F,
Time 10.0 hour
0.2% creep
 23.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
3340 psi
@Temperature 599 °F,
Time 1000 hour
0.1% creep
 27.0 MPa
@Temperature 370 °C,
Time 36000 sec
3920 psi
@Temperature 698 °F,
Time 10.0 hour
0.5% creep
 28.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
4060 psi
@Temperature 599 °F,
Time 1000 hour
0.2% creep
 30.0 MPa
@Temperature 370 °C,
Time 36000 sec
4350 psi
@Temperature 698 °F,
Time 10.0 hour
1% creep
 32.0 MPa
@Temperature 370 °C,
Time 3600 sec
4640 psi
@Temperature 698 °F,
Time 1.00 hour
0.1% creep
 38.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
5510 psi
@Temperature 599 °F,
Time 1000 hour
0.5% creep
 38.0 MPa
@Temperature 315 °C,
Time 360000 sec
5510 psi
@Temperature 599 °F,
Time 100 hour
0.1% creep
 41.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
5950 psi
@Temperature 599 °F,
Time 1000 hour
1% creep
 45.0 MPa
@Temperature 370 °C,
Time 3600 sec
6530 psi
@Temperature 698 °F,
Time 1.00 hour
0.2% creep
 52.0 MPa
@Temperature 315 °C,
Time 360000 sec
7540 psi
@Temperature 599 °F,
Time 100 hour
0.2% creep
 59.0 MPa
@Temperature 370 °C,
Time 3600 sec
8560 psi
@Temperature 698 °F,
Time 1.00 hour
0.5% creep
 59.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
8560 psi
@Temperature 500 °F,
Time 1000 hour
0.1% creep
 62.0 MPa
@Temperature 370 °C,
Time 3600 sec
8990 psi
@Temperature 698 °F,
Time 1.00 hour
1% creep
 62.0 MPa
@Temperature 315 °C,
Time 360000 sec
8990 psi
@Temperature 599 °F,
Time 100 hour
0.5% creep
 62.0 MPa
@Temperature 315 °C,
Time 36000 sec
8990 psi
@Temperature 599 °F,
Time 10.0 hour
0.1% creep
 66.0 MPa
@Temperature 370 °C,
Time 360 sec
9570 psi
@Temperature 698 °F,
Time 0.100 hour
0.2% creep
 66.0 MPa
@Temperature 370 °C,
Time 360 sec
9570 psi
@Temperature 698 °F,
Time 0.100 hour
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 360000 sec
10000 psi
@Temperature 500 °F,
Time 100 hour
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+7 sec
10000 psi
@Temperature 500 °F,
Time 10000 hour
1% creep
 69.0 MPa
@Temperature 315 °C,
Time 360000 sec
10000 psi
@Temperature 599 °F,
Time 100 hour
1% creep
 69.0 MPa
@Temperature 370 °C,
Time 360 sec
10000 psi
@Temperature 698 °F,
Time 0.100 hour
1% creep
 69.0 MPa
@Temperature 370 °C,
Time 360 sec
10000 psi
@Temperature 698 °F,
Time 0.100 hour
0.5% creep
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
10000 psi
@Temperature 500 °F,
Time 1000 hour
0.2% creep
 69.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
10000 psi
@Temperature 446 °F,
Time 1000 hour
0.1% creep
 76.0 MPa
@Temperature 315 °C,
Time 36000 sec
11000 psi
@Temperature 599 °F,
Time 10.0 hour
0.2% creep
 83.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
12000 psi
@Temperature 500 °F,
Time 1000 hour
0.5% creep
 90.0 MPa
@Temperature 315 °C,
Time 36000 sec
13100 psi
@Temperature 599 °F,
Time 10.0 hour
0.5% creep
 90.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
13100 psi
@Temperature 446 °F,
Time 1000 hour
0.2% creep
 90.0 MPa
@Temperature 260 °C,
Time 360000 sec
13100 psi
@Temperature 500 °F,
Time 100 hour
0.2% creep
 90.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
13100 psi
@Temperature 401 °F,
Time 1000 hour
0.1% creep
 90.0 MPa
@Temperature 230 °C,
Time 360000 sec
13100 psi
@Temperature 446 °F,
Time 100 hour
0.1% creep
 90.0 MPa
@Temperature 260 °C,
Time 36000 sec
13100 psi
@Temperature 500 °F,
Time 10.0 hour
0.1% creep
 90.0 MPa
@Temperature 315 °C,
Time 3600 sec
13100 psi
@Temperature 599 °F,
Time 1.00 hour
0.1% creep
 97.0 MPa
@Temperature 230 °C,
Time 3.60e+7 sec
14100 psi
@Temperature 446 °F,
Time 10000 hour
1% creep
 97.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
14100 psi
@Temperature 500 °F,
Time 1000 hour
1% creep
 97.0 MPa
@Temperature 315 °C,
Time 36000 sec
14100 psi
@Temperature 599 °F,
Time 10.0 hour
1% creep
 97.0 MPa
@Temperature 230 °C,
Time 3.60e+7 sec
14100 psi
@Temperature 446 °F,
Time 10000 hour
0.5% creep
 105 MPa
@Temperature 315 °C,
Time 3600 sec
15200 psi
@Temperature 599 °F,
Time 1.00 hour
0.2% creep
 105 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
15200 psi
@Temperature 347 °F,
Time 1000 hour
0.1% creep
 110 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
16000 psi
@Temperature 446 °F,
Time 1000 hour
0.5% creep
 110 MPa
@Temperature 260 °C,
Time 360000 sec
16000 psi
@Temperature 500 °F,
Time 100 hour
0.5% creep
 110 MPa
@Temperature 315 °C,
Time 3600 sec
16000 psi
@Temperature 599 °F,
Time 1.00 hour
0.5% creep
 110 MPa
@Temperature 230 °C,
Time 360000 sec
16000 psi
@Temperature 446 °F,
Time 100 hour
0.2% creep
 110 MPa
@Temperature 260 °C,
Time 36000 sec
16000 psi
@Temperature 500 °F,
Time 10.0 hour
0.2% creep
 110 MPa
@Temperature 205 °C,
Time 360000 sec
16000 psi
@Temperature 401 °F,
Time 100 hour
0.1% creep
 110 MPa
@Temperature 230 °C,
Time 36000 sec
16000 psi
@Temperature 446 °F,
Time 10.0 hour
0.1% creep
 110 MPa
@Temperature 315 °C,
Time 360 sec
16000 psi
@Temperature 599 °F,
Time 0.100 hour
0.1% creep
 115 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
16700 psi
@Temperature 446 °F,
Time 1000 hour
1% creep
 115 MPa
@Temperature 315 °C,
Time 3600 sec
16700 psi
@Temperature 599 °F,
Time 1.00 hour
1% creep
 115 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
16700 psi
@Temperature 401 °F,
Time 1000 hour
0.2% creep
 115 MPa
@Temperature 315 °C,
Time 360 sec
16700 psi
@Temperature 599 °F,
Time 0.100 hour
0.2% creep
 115 MPa
@Temperature 260 °C,
Time 3600 sec
16700 psi
@Temperature 500 °F,
Time 1.00 hour
0.1% creep
 125 MPa
@Temperature 205 °C,
Time 3.60e+7 sec
18100 psi
@Temperature 401 °F,
Time 10000 hour
1% creep
 125 MPa
@Temperature 260 °C,
Time 360000 sec
18100 psi
@Temperature 500 °F,
Time 100 hour
1% creep
 125 MPa
@Temperature 315 °C,
Time 360 sec
18100 psi
@Temperature 599 °F,
Time 0.100 hour
1% creep
 125 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
18100 psi
@Temperature 401 °F,
Time 1000 hour
0.5% creep
 125 MPa
@Temperature 315 °C,
Time 360 sec
18100 psi
@Temperature 599 °F,
Time 0.100 hour
0.5% creep
 130 MPa
@Temperature 230 °C,
Time 360000 sec
18900 psi
@Temperature 446 °F,
Time 100 hour
0.5% creep
 130 MPa
@Temperature 260 °C,
Time 36000 sec
18900 psi
@Temperature 500 °F,
Time 10.0 hour
0.5% creep
 130 MPa
@Temperature 205 °C,
Time 360000 sec
18900 psi
@Temperature 401 °F,
Time 100 hour
0.2% creep
 130 MPa
@Temperature 230 °C,
Time 36000 sec
18900 psi
@Temperature 446 °F,
Time 10.0 hour
0.2% creep
 130 MPa
@Temperature 175 °C,
Time 360000 sec
18900 psi
@Temperature 347 °F,
Time 100 hour
0.1% creep
 130 MPa
@Temperature 205 °C,
Time 36000 sec
18900 psi
@Temperature 401 °F,
Time 10.0 hour
0.1% creep
 140 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
20300 psi
@Temperature 401 °F,
Time 1000 hour
1% creep
 140 MPa
@Temperature 230 °C,
Time 360000 sec
20300 psi
@Temperature 446 °F,
Time 100 hour
1% creep
 140 MPa
@Temperature 260 °C,
Time 36000 sec
20300 psi
@Temperature 500 °F,
Time 10.0 hour
1% creep
 140 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
20300 psi
@Temperature 347 °F,
Time 1000 hour
0.2% creep
 140 MPa
@Temperature 260 °C,
Time 3600 sec
20300 psi
@Temperature 500 °F,
Time 1.00 hour
0.2% creep
 140 MPa
@Temperature 230 °C,
Time 3600 sec
20300 psi
@Temperature 446 °F,
Time 1.00 hour
0.1% creep
 145 MPa
@Temperature 260 °C,
Time 360 sec
21000 psi
@Temperature 500 °F,
Time 0.100 hour
0.1% creep
 150 MPa
@Temperature 205 °C,
Time 360000 sec
21800 psi
@Temperature 401 °F,
Time 100 hour
0.5% creep
 150 MPa
@Temperature 230 °C,
Time 36000 sec
21800 psi
@Temperature 446 °F,
Time 10.0 hour
0.5% creep
 150 MPa
@Temperature 260 °C,
Time 3600 sec
21800 psi
@Temperature 500 °F,
Time 1.00 hour
0.5% creep
 150 MPa
@Temperature 205 °C,
Time 36000 sec
21800 psi
@Temperature 401 °F,
Time 10.0 hour
0.2% creep
 150 MPa
@Temperature 230 °C,
Time 3600 sec
21800 psi
@Temperature 446 °F,
Time 1.00 hour
0.2% creep
 150 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
21800 psi
@Temperature 302 °F,
Time 1000 hour
0.1% creep
 160 MPa
@Temperature 230 °C,
Time 36000 sec
23200 psi
@Temperature 446 °F,
Time 10.0 hour
1% creep
 160 MPa
@Temperature 260 °C,
Time 3600 sec
23200 psi
@Temperature 500 °F,
Time 1.00 hour
1% creep
 160 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
23200 psi
@Temperature 347 °F,
Time 1000 hour
0.5% creep
 160 MPa
@Temperature 175 °C,
Time 360000 sec
23200 psi
@Temperature 347 °F,
Time 100 hour
0.2% creep
 160 MPa
@Temperature 260 °C,
Time 360 sec
23200 psi
@Temperature 500 °F,
Time 0.100 hour
0.2% creep
 160 MPa
@Temperature 205 °C,
Time 3600 sec
23200 psi
@Temperature 401 °F,
Time 1.00 hour
0.1% creep
 165 MPa
@Temperature 205 °C,
Time 360000 sec
23900 psi
@Temperature 401 °F,
Time 100 hour
1% creep
 165 MPa
@Temperature 260 °C,
Time 360 sec
23900 psi
@Temperature 500 °F,
Time 0.100 hour
0.5% creep
 165 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
23900 psi
@Temperature 302 °F,
Time 1000 hour
0.2% creep
 165 MPa
@Temperature 175 °C,
Time 36000 sec
23900 psi
@Temperature 347 °F,
Time 10.0 hour
0.1% creep
 165 MPa
@Temperature 230 °C,
Time 360 sec
23900 psi
@Temperature 446 °F,
Time 0.100 hour
0.1% creep
 170 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
24700 psi
@Temperature 347 °F,
Time 1000 hour
1% creep
 170 MPa
@Temperature 260 °C,
Time 360 sec
24700 psi
@Temperature 500 °F,
Time 0.100 hour
1% creep
 170 MPa
@Temperature 230 °C,
Time 3600 sec
24700 psi
@Temperature 446 °F,
Time 1.00 hour
0.5% creep
 170 MPa
@Temperature 150 °C,
Time 360000 sec
24700 psi
@Temperature 302 °F,
Time 100 hour
0.1% creep
 180 MPa
@Temperature 205 °C,
Time 36000 sec
26100 psi
@Temperature 401 °F,
Time 10.0 hour
0.5% creep
 180 MPa
@Temperature 205 °C,
Time 3600 sec
26100 psi
@Temperature 401 °F,
Time 1.00 hour
0.2% creep
 180 MPa
@Temperature 230 °C,
Time 360 sec
26100 psi
@Temperature 446 °F,
Time 0.100 hour
0.2% creep
 185 MPa
@Temperature 230 °C,
Time 3600 sec
26800 psi
@Temperature 446 °F,
Time 1.00 hour
1% creep
 185 MPa
@Temperature 175 °C,
Time 360000 sec
26800 psi
@Temperature 347 °F,
Time 100 hour
0.5% creep
 195 MPa
@Temperature 205 °C,
Time 36000 sec
28300 psi
@Temperature 401 °F,
Time 10.0 hour
1% creep
 195 MPa
@Temperature 175 °C,
Time 36000 sec
28300 psi
@Temperature 347 °F,
Time 10.0 hour
0.2% creep
 195 MPa
@Temperature 205 °C,
Time 360 sec
28300 psi
@Temperature 401 °F,
Time 0.100 hour
0.1% creep
 200 MPa
@Temperature 175 °C,
Time 360000 sec
29000 psi
@Temperature 347 °F,
Time 100 hour
1% creep
 200 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
29000 psi
@Temperature 302 °F,
Time 1000 hour
0.5% creep
 200 MPa
@Temperature 230 °C,
Time 360 sec
29000 psi
@Temperature 446 °F,
Time 0.100 hour
0.5% creep
 200 MPa
@Temperature 150 °C,
Time 360000 sec
29000 psi
@Temperature 302 °F,
Time 100 hour
0.2% creep
 200 MPa
@Temperature 175 °C,
Time 3600 sec
29000 psi
@Temperature 347 °F,
Time 1.00 hour
0.1% creep
 205 MPa
@Temperature 230 °C,
Time 360 sec
29700 psi
@Temperature 446 °F,
Time 0.100 hour
1% creep
 205 MPa
@Temperature 205 °C,
Time 3600 sec
29700 psi
@Temperature 401 °F,
Time 1.00 hour
0.5% creep
 205 MPa
@Temperature 150 °C,
Time 36000 sec
29700 psi
@Temperature 302 °F,
Time 10.0 hour
0.1% creep
 215 MPa
@Temperature 175 °C,
Time 36000 sec
31200 psi
@Temperature 347 °F,
Time 10.0 hour
0.5% creep
 215 MPa
@Temperature 205 °C,
Time 360 sec
31200 psi
@Temperature 401 °F,
Time 0.100 hour
0.2% creep
 220 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
31900 psi
@Temperature 302 °F,
Time 1000 hour
1% creep
 220 MPa
@Temperature 205 °C,
Time 3600 sec
31900 psi
@Temperature 401 °F,
Time 1.00 hour
1% creep
 220 MPa
@Temperature 175 °C,
Time 3600 sec
31900 psi
@Temperature 347 °F,
Time 1.00 hour
0.2% creep
 230 MPa
@Temperature 175 °C,
Time 36000 sec
33400 psi
@Temperature 347 °F,
Time 10.0 hour
1% creep
 230 MPa
@Temperature 175 °C,
Time 360 sec
33400 psi
@Temperature 347 °F,
Time 0.100 hour
0.1% creep
 235 MPa
@Temperature 150 °C,
Time 360000 sec
34100 psi
@Temperature 302 °F,
Time 100 hour
0.5% creep
 235 MPa
@Temperature 205 °C,
Time 360 sec
34100 psi
@Temperature 401 °F,
Time 0.100 hour
0.5% creep
 235 MPa
@Temperature 150 °C,
Time 36000 sec
34100 psi
@Temperature 302 °F,
Time 10.0 hour
0.2% creep
 235 MPa
@Temperature 150 °C,
Time 3600 sec
34100 psi
@Temperature 302 °F,
Time 1.00 hour
0.1% creep
 240 MPa
@Temperature 205 °C,
Time 360 sec
34800 psi
@Temperature 401 °F,
Time 0.100 hour
1% creep
 240 MPa
@Temperature 175 °C,
Time 3600 sec
34800 psi
@Temperature 347 °F,
Time 1.00 hour
0.5% creep
 250 MPa
@Temperature 150 °C,
Time 360000 sec
36300 psi
@Temperature 302 °F,
Time 100 hour
1% creep
 250 MPa
@Temperature 175 °C,
Time 360 sec
36300 psi
@Temperature 347 °F,
Time 0.100 hour
0.2% creep
 255 MPa
@Temperature 175 °C,
Time 3600 sec
37000 psi
@Temperature 347 °F,
Time 1.00 hour
1% creep
 255 MPa
@Temperature 150 °C,
Time 36000 sec
37000 psi
@Temperature 302 °F,
Time 10.0 hour
0.5% creep
 255 MPa
@Temperature 150 °C,
Time 3600 sec
37000 psi
@Temperature 302 °F,
Time 1.00 hour
0.2% creep
 260 MPa
@Temperature 175 °C,
Time 360 sec
37700 psi
@Temperature 347 °F,
Time 0.100 hour
0.5% creep
 260 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
37700 psi
@Temperature 212 °F,
Time 1000 hour
0.1% creep
 260 MPa
@Temperature 150 °C,
Time 360 sec
37700 psi
@Temperature 302 °F,
Time 0.100 hour
0.1% creep
 270 MPa
@Temperature 150 °C,
Time 36000 sec
39200 psi
@Temperature 302 °F,
Time 10.0 hour
1% creep
 270 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
39200 psi
@Temperature 212 °F,
Time 1000 hour
0.2% creep
 270 MPa
@Temperature 100 °C,
Time 360000 sec
39200 psi
@Temperature 212 °F,
Time 100 hour
0.1% creep
 275 MPa
@Temperature 175 °C,
Time 360 sec
39900 psi
@Temperature 347 °F,
Time 0.100 hour
1% creep
 275 MPa
@Temperature 150 °C,
Time 3600 sec
39900 psi
@Temperature 302 °F,
Time 1.00 hour
0.5% creep
 275 MPa
@Temperature 100 °C,
Time 360000 sec
39900 psi
@Temperature 212 °F,
Time 100 hour
0.2% creep
 275 MPa
@Temperature 150 °C,
Time 360 sec
39900 psi
@Temperature 302 °F,
Time 0.100 hour
0.2% creep
 275 MPa
@Temperature 100 °C,
Time 36000 sec
39900 psi
@Temperature 212 °F,
Time 10.0 hour
0.1% creep
 285 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
41300 psi
@Temperature 212 °F,
Time 1000 hour
0.5% creep
 285 MPa
@Temperature 100 °C,
Time 3600 sec
41300 psi
@Temperature 212 °F,
Time 1.00 hour
0.1% creep
 290 MPa
@Temperature 150 °C,
Time 3600 sec
42100 psi
@Temperature 302 °F,
Time 1.00 hour
1% creep
 290 MPa
@Temperature 100 °C,
Time 36000 sec
42100 psi
@Temperature 212 °F,
Time 10.0 hour
0.2% creep
 295 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
42800 psi
@Temperature 212 °F,
Time 1000 hour
1% creep
 295 MPa
@Temperature 100 °C,
Time 360000 sec
42800 psi
@Temperature 212 °F,
Time 100 hour
0.5% creep
 295 MPa
@Temperature 150 °C,
Time 360 sec
42800 psi
@Temperature 302 °F,
Time 0.100 hour
0.5% creep
 305 MPa
@Temperature 150 °C,
Time 360 sec
44200 psi
@Temperature 302 °F,
Time 0.100 hour
1% creep
 305 MPa
@Temperature 100 °C,
Time 3600 sec
44200 psi
@Temperature 212 °F,
Time 1.00 hour
0.2% creep
 305 MPa
@Temperature 100 °C,
Time 360 sec
44200 psi
@Temperature 212 °F,
Time 0.100 hour
0.1% creep
 310 MPa
@Temperature 100 °C,
Time 360000 sec
45000 psi
@Temperature 212 °F,
Time 100 hour
1% creep
 310 MPa
@Temperature 100 °C,
Time 36000 sec
45000 psi
@Temperature 212 °F,
Time 10.0 hour
0.5% creep
 315 MPa
@Temperature 100 °C,
Time 360 sec
45700 psi
@Temperature 212 °F,
Time 0.100 hour
0.2% creep
 315 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
45700 psi
@Temperature 75.2 °F,
Time 1000 hour
0.1% creep
 325 MPa
@Temperature 100 °C,
Time 36000 sec
47100 psi
@Temperature 212 °F,
Time 10.0 hour
1% creep
 325 MPa
@Temperature 100 °C,
Time 3600 sec
47100 psi
@Temperature 212 °F,
Time 1.00 hour
0.5% creep
 325 MPa
@Temperature 24.0 °C,
Time 360000 sec
47100 psi
@Temperature 75.2 °F,
Time 100 hour
0.1% creep
 330 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
47900 psi
@Temperature 75.2 °F,
Time 1000 hour
0.2% creep
 330 MPa
@Temperature 24.0 °C,
Time 36000 sec
47900 psi
@Temperature 75.2 °F,
Time 10.0 hour
0.1% creep
 340 MPa
@Temperature 100 °C,
Time 3600 sec
49300 psi
@Temperature 212 °F,
Time 1.00 hour
1% creep
 340 MPa
@Temperature 100 °C,
Time 360 sec
49300 psi
@Temperature 212 °F,
Time 0.100 hour
0.5% creep
 340 MPa
@Temperature 24.0 °C,
Time 360000 sec
49300 psi
@Temperature 75.2 °F,
Time 100 hour
0.2% creep
 345 MPa
@Temperature 24.0 °C,
Time 36000 sec
50000 psi
@Temperature 75.2 °F,
Time 10.0 hour
0.2% creep
 345 MPa
@Temperature 24.0 °C,
Time 3600 sec
50000 psi
@Temperature 75.2 °F,
Time 1.00 hour
0.1% creep
 350 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
50800 psi
@Temperature 75.2 °F,
Time 1000 hour
0.5% creep
 350 MPa
@Temperature 24.0 °C,
Time 360 sec
50800 psi
@Temperature 75.2 °F,
Time 0.100 hour
0.1% creep
 360 MPa
@Temperature 100 °C,
Time 360 sec
52200 psi
@Temperature 212 °F,
Time 0.100 hour
1% creep
 360 MPa
@Temperature 24.0 °C,
Time 360000 sec
52200 psi
@Temperature 75.2 °F,
Time 100 hour
0.5% creep
 360 MPa
@Temperature 24.0 °C,
Time 3600 sec
52200 psi
@Temperature 75.2 °F,
Time 1.00 hour
0.2% creep
 365 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
52900 psi
@Temperature 75.2 °F,
Time 1000 hour
1% creep
 365 MPa
@Temperature 24.0 °C,
Time 36000 sec
52900 psi
@Temperature 75.2 °F,
Time 10.0 hour
0.5% creep
 365 MPa
@Temperature 24.0 °C,
Time 360 sec
52900 psi
@Temperature 75.2 °F,
Time 0.100 hour
0.2% creep
 380 MPa
@Temperature 24.0 °C,
Time 360000 sec
55100 psi
@Temperature 75.2 °F,
Time 100 hour
1% creep
 385 MPa
@Temperature 24.0 °C,
Time 3600 sec
55800 psi
@Temperature 75.2 °F,
Time 1.00 hour
0.5% creep
 400 MPa
@Temperature 24.0 °C,
Time 36000 sec
58000 psi
@Temperature 75.2 °F,
Time 10.0 hour
1% creep
 415 MPa
@Temperature 24.0 °C,
Time 360 sec
60200 psi
@Temperature 75.2 °F,
Time 0.100 hour
0.5% creep
 420 MPa
@Temperature 24.0 °C,
Time 3600 sec
60900 psi
@Temperature 75.2 °F,
Time 1.00 hour
1% creep
 435 MPa
@Temperature 24.0 °C,
Time 360 sec
63100 psi
@Temperature 75.2 °F,
Time 0.100 hour
1% creep
Rupture Strength  14.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
2030 psi
@Temperature 698 °F,
Time 1000 hour
 22.0 MPa
@Temperature 315 °C,
Time 3.60e+7 sec
3190 psi
@Temperature 599 °F,
Time 10000 hour
 22.0 MPa
@Temperature 370 °C,
Time 360000 sec
3190 psi
@Temperature 698 °F,
Time 100 hour
 32.0 MPa
@Temperature 370 °C,
Time 36000 sec
4640 psi
@Temperature 698 °F,
Time 10.0 hour
 41.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
5950 psi
@Temperature 599 °F,
Time 1000 hour
 45.0 MPa
@Temperature 260 °C,
Time 3.60e+8 sec
6530 psi
@Temperature 500 °F,
Time 100000 hour
 62.0 MPa
@Temperature 370 °C,
Time 3600 sec
8990 psi
@Temperature 698 °F,
Time 1.00 hour
 66.0 MPa
@Temperature 230 °C,
Time 3.60e+8 sec
9570 psi
@Temperature 446 °F,
Time 100000 hour
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+7 sec
10000 psi
@Temperature 500 °F,
Time 10000 hour
 69.0 MPa
@Temperature 315 °C,
Time 360000 sec
10000 psi
@Temperature 599 °F,
Time 100 hour
 69.0 MPa
@Temperature 370 °C,
Time 360 sec
10000 psi
@Temperature 698 °F,
Time 0.100 hour
 97.0 MPa
@Temperature 205 °C,
Time 3.60e+8 sec
14100 psi
@Temperature 401 °F,
Time 100000 hour
 97.0 MPa
@Temperature 230 °C,
Time 3.60e+7 sec
14100 psi
@Temperature 446 °F,
Time 10000 hour
 105 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
15200 psi
@Temperature 500 °F,
Time 1000 hour
 105 MPa
@Temperature 315 °C,
Time 36000 sec
15200 psi
@Temperature 599 °F,
Time 10.0 hour
 115 MPa
@Temperature 315 °C,
Time 3600 sec
16700 psi
@Temperature 599 °F,
Time 1.00 hour
 125 MPa
@Temperature 205 °C,
Time 3.60e+7 sec
18100 psi
@Temperature 401 °F,
Time 10000 hour
 125 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
18100 psi
@Temperature 446 °F,
Time 1000 hour
 130 MPa
@Temperature 175 °C,
Time 3.60e+8 sec
18900 psi
@Temperature 347 °F,
Time 100000 hour
 130 MPa
@Temperature 260 °C,
Time 360000 sec
18900 psi
@Temperature 500 °F,
Time 100 hour
 130 MPa
@Temperature 315 °C,
Time 360 sec
18900 psi
@Temperature 599 °F,
Time 0.100 hour
 150 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
21800 psi
@Temperature 401 °F,
Time 1000 hour
 150 MPa
@Temperature 230 °C,
Time 360000 sec
21800 psi
@Temperature 446 °F,
Time 100 hour
 150 MPa
@Temperature 260 °C,
Time 36000 sec
21800 psi
@Temperature 500 °F,
Time 10.0 hour
 160 MPa
@Temperature 175 °C,
Time 3.60e+7 sec
23200 psi
@Temperature 347 °F,
Time 10000 hour
 165 MPa
@Temperature 260 °C,
Time 3600 sec
23900 psi
@Temperature 500 °F,
Time 1.00 hour
 170 MPa
@Temperature 150 °C,
Time 3.60e+8 sec
24700 psi
@Temperature 302 °F,
Time 100000 hour
 170 MPa
@Temperature 230 °C,
Time 36000 sec
24700 psi
@Temperature 446 °F,
Time 10.0 hour
 180 MPa
@Temperature 205 °C,
Time 360000 sec
26100 psi
@Temperature 401 °F,
Time 100 hour
 180 MPa
@Temperature 260 °C,
Time 360 sec
26100 psi
@Temperature 500 °F,
Time 0.100 hour
 185 MPa
@Temperature 175 °C,
Time 3.60e+6 sec
26800 psi
@Temperature 347 °F,
Time 1000 hour
 200 MPa
@Temperature 230 °C,
Time 3600 sec
29000 psi
@Temperature 446 °F,
Time 1.00 hour
 205 MPa
@Temperature 150 °C,
Time 3.60e+7 sec
29700 psi
@Temperature 302 °F,
Time 10000 hour
 205 MPa
@Temperature 205 °C,
Time 36000 sec
29700 psi
@Temperature 401 °F,
Time 10.0 hour
 220 MPa
@Temperature 175 °C,
Time 360000 sec
31900 psi
@Temperature 347 °F,
Time 100 hour
 230 MPa
@Temperature 230 °C,
Time 360 sec
33400 psi
@Temperature 446 °F,
Time 0.100 hour
 235 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
34100 psi
@Temperature 302 °F,
Time 1000 hour
 235 MPa
@Temperature 205 °C,
Time 3600 sec
34100 psi
@Temperature 401 °F,
Time 1.00 hour
 250 MPa
@Temperature 175 °C,
Time 36000 sec
36300 psi
@Temperature 347 °F,
Time 10.0 hour
 260 MPa
@Temperature 150 °C,
Time 360000 sec
37700 psi
@Temperature 302 °F,
Time 100 hour
 270 MPa
@Temperature 205 °C,
Time 360 sec
39200 psi
@Temperature 401 °F,
Time 0.100 hour
 275 MPa
@Temperature 175 °C,
Time 3600 sec
39900 psi
@Temperature 347 °F,
Time 1.00 hour
 290 MPa
@Temperature 150 °C,
Time 36000 sec
42100 psi
@Temperature 302 °F,
Time 10.0 hour
 305 MPa
@Temperature 175 °C,
Time 360 sec
44200 psi
@Temperature 347 °F,
Time 0.100 hour
 315 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
45700 psi
@Temperature 212 °F,
Time 1000 hour
 315 MPa
@Temperature 150 °C,
Time 3600 sec
45700 psi
@Temperature 302 °F,
Time 1.00 hour
 330 MPa
@Temperature 100 °C,
Time 360000 sec
47900 psi
@Temperature 212 °F,
Time 100 hour
 340 MPa
@Temperature 150 °C,
Time 360 sec
49300 psi
@Temperature 302 °F,
Time 0.100 hour
 350 MPa
@Temperature 100 °C,
Time 36000 sec
50800 psi
@Temperature 212 °F,
Time 10.0 hour
 370 MPa
@Temperature 100 °C,
Time 3600 sec
53700 psi
@Temperature 212 °F,
Time 1.00 hour
 395 MPa
@Temperature 100 °C,
Time 360 sec
57300 psi
@Temperature 212 °F,
Time 0.100 hour
 420 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
60900 psi
@Temperature 75.2 °F,
Time 1000 hour
 425 MPa
@Temperature 24.0 °C,
Time 360000 sec
61600 psi
@Temperature 75.2 °F,
Time 100 hour
 435 MPa
@Temperature 24.0 °C,
Time 36000 sec
63100 psi
@Temperature 75.2 °F,
Time 10.0 hour
 450 MPa
@Temperature 24.0 °C,
Time 3600 sec
65300 psi
@Temperature 75.2 °F,
Time 1.00 hour
 455 MPa
@Temperature 24.0 °C,
Time 360 sec
66000 psi
@Temperature 75.2 °F,
Time 0.100 hour
Modulus of Elasticity 73.1 GPa10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Fatigue Strength 103 MPa
@# of Cycles 5.00e+8
15000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPa3920 ksiEstimated from similar Al alloys.
Shear Strength 285 MPa41300 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000570 ohm-cm0.00000570 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
11.6 µin/in-°F
@Temperature -58.0 - 68.0 °F
 22.3 µm/m-°C
@Temperature 20.0 - 100 °C
12.4 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
12.5 µin/in-°F
@Temperature 68.0 - 212 °F
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.0 µin/in-°F
@Temperature 68.0 - 392 °F
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
13.4 µin/in-°F
@Temperature 68.0 - 572 °F
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
13.6 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.864 J/g-°C0.207 BTU/lb-°F
Thermal Conductivity 120 W/m-K833 BTU-in/hr-ft²-°F
Melting Point 543 - 643 °C1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 543 °C1010 °FAA; Typical
Liquidus 643 °C1190 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 535 °C995 °F
Aging Temperature 163 - 191 °C325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 91.5 - 93.8 %91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %5.8 - 6.8 %
Iron, Fe <= 0.30 %<= 0.30 %
Magnesium, Mg <= 0.02 %<= 0.02 %
Manganese, Mn 0.20 - 0.40 %0.20 - 0.40 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.20 %<= 0.20 %
Titanium, Ti 0.02 - 0.10 %0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %0.05 - 0.15 %
Zinc, Zn <= 0.10 %<= 0.10 %
Zirconium, Zr 0.10 - 0.25 %0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2219-T81
Aluminum 2219-T62
Aluminum 2219-T851
Aluminum 2014-T6; 2014-T651
302 Stainless Steel, 60% cold reduction

MA2219T851a / 170633

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.