MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Titanium Grade 3
Categories: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium

Material Notes: Information provided by Allvac and the references.

Characterized by: good fabrication properties and intermediate strength

Applications: Airframe skin, heat exchangers, cryogenic vessels, components for CPI equipment, condenser tubing, exhaust pipe shrouds.

Forms typically available: billet, bar, plate, sheet, strip, rod, wire, extrusions, tubing.

Titanium Grades 1,2,3,4,7,11,and 12 are all considered unalloyed and have similar mechanical properties.

Key Words: ASTM Grade 3; UNS R50550, CP titanium, C.P. titanium alloy
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.50 g/cc0.163 lb/in³
 
Chemical PropertiesMetricEnglishComments
Thermal Neutron Cross Section 5.6 barns/atom5.6 barns/atomNaturally occurring Ti
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 225225annealed
Hardness, Knoop 175175unwelded sample
 220220welded
Hardness, Rockwell B 9090annealed
Hardness, Rockwell C 1616Estimated from Brinell.
Tensile Strength  165 MPa
@Temperature 538 °C
23900 psi
@Temperature 1000 °F
 250 MPa
@Temperature 316 °C
36300 psi
@Temperature 601 °F
 440 MPa
@Temperature 93.0 °C
63800 psi
@Temperature 199 °F
 690 MPa
@Temperature -54.0 °C
100000 psi
@Temperature -65.2 °F
 1210 MPa
@Temperature -253 °C
175000 psi
@Temperature -423 °F
Tensile Strength, Ultimate 440 MPa63800 psi
Tensile Strength, Yield 377 - 520 MPa54700 - 75400 psi
 90.0 MPa
@Temperature 538 °C
13100 psi
@Temperature 1000 °F
0.2% offset
 140 MPa
@Temperature 316 °C
20300 psi
@Temperature 601 °F
0.2% offset
 340 MPa
@Temperature 93.0 °C
49300 psi
@Temperature 199 °F
0.2% offset
 450 MPa
@Temperature 21.0 °C
65300 psi
@Temperature 69.8 °F
0.2% offset
 510 MPa
@Temperature -54.0 °C
74000 psi
@Temperature -65.2 °F
0.2% offset
Elongation at Break 25 %25 %
Reduction of Area 50 %50 %
Tensile Modulus 107 GPa15500 ksi
Compressive Yield Strength 450 MPa65300 psi0.2% offset
 140 MPa
@Temperature 538 °C
20300 psi
@Temperature 1000 °F
 200 MPa
@Temperature 316 °C
29000 psi
@Temperature 601 °F
 315 MPa
@Temperature 93.0 °C
45700 psi
@Temperature 199 °F
Compressive Modulus 107 GPa15500 ksi
Ultimate Bearing Strength 1000 MPa145000 psiCold Worked
 180 MPa
@Temperature 538 °C
26100 psi
@Temperature 1000 °F
 345 MPa
@Temperature 316 °C
50000 psi
@Temperature 601 °F
 580 MPa
@Temperature 93.0 °C
84100 psi
@Temperature 199 °F
 680 MPa
@Temperature 21.0 °C
98600 psi
@Temperature 69.8 °F
Bearing Yield Strength 900 MPa131000 psiCold Worked
 145 MPa
@Temperature 538 °C
21000 psi
@Temperature 1000 °F
2% permanent set.
 240 MPa
@Temperature 316 °C
34800 psi
@Temperature 601 °F
2% permanent set.
 455 MPa
@Temperature 93.0 °C
66000 psi
@Temperature 199 °F
2% permanent set.
 565 MPa
@Temperature 21.0 °C
81900 psi
@Temperature 69.8 °F
2% permanent set.
Poissons Ratio 0.330.33
Fatigue Strength  240 MPa
@# of Cycles 1.00e+7
34800 psi
@# of Cycles 1.00e+7
R = -1
 289 MPa
@# of Cycles 1.00e+6
41900 psi
@# of Cycles 1.00e+6
 305 MPa
@# of Cycles 1.00e+7
44200 psi
@# of Cycles 1.00e+7
Cold rolled
 315 MPa
@# of Cycles 1.00e+6
45700 psi
@# of Cycles 1.00e+6
Cold rolled
 325 MPa
@# of Cycles 100000
47100 psi
@# of Cycles 100000
Cold rolled
 420 MPa
@# of Cycles 10000
60900 psi
@# of Cycles 10000
Cold rolled
Fracture Toughness 79.0 MPa-m½71.9 ksi-in½for K(Q) after anneal
Shear Modulus 41.0 GPa5950 ksi
Shear Strength  110 MPa
@Temperature 538 °C
16000 psi
@Temperature 1000 °F
 195 MPa
@Temperature 316 °C
28300 psi
@Temperature 601 °F
 315 MPa
@Temperature 93.0 °C
45700 psi
@Temperature 199 °F
 380 MPa
@Temperature 21.0 °C
55100 psi
@Temperature 69.8 °F
Charpy Impact 30.0 - 66.0 J22.1 - 48.7 ft-lbV-notch; also reported as 40 J
 60.0 J
@Temperature 0.000 °C
44.3 ft-lb
@Temperature 32.0 °F
Notched
 70.0 J
@Temperature 100 °C
51.6 ft-lb
@Temperature 212 °F
Notched
 85.0 J
@Temperature 200 °C
62.7 ft-lb
@Temperature 392 °F
Notched
 95.0 J
@Temperature 300 °C
70.1 ft-lb
@Temperature 572 °F
Notched
Coefficient of Friction, Dynamic 0.680.68Ti sliding on Ti; 300 m/min
 0.800.80Ti sliding on Ti; 40 m/min
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000540 ohm-cm0.0000540 ohm-cm
 0.0000900 ohm-cm
@Temperature 250 °C
0.0000900 ohm-cm
@Temperature 482 °F
 0.000120 ohm-cm
@Temperature 500 °C
0.000120 ohm-cm
@Temperature 932 °F
 0.000150 ohm-cm
@Temperature 750 °C
0.000150 ohm-cm
@Temperature 1380 °F
Magnetic Permeability 1.000051.00005at 1.6 kA/m
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 325 J/g140 BTU/lbHigh Purity Ti.
CTE, linear  8.60 µm/m-°C
@Temperature 0.000 - 100 °C
4.78 µin/in-°F
@Temperature 32.0 - 212 °F
 9.20 µm/m-°C
@Temperature 0.000 - 315 °C
5.11 µin/in-°F
@Temperature 32.0 - 599 °F
average
 9.70 µm/m-°C
@Temperature 0.000 - 540 °C
5.39 µin/in-°F
@Temperature 32.0 - 1000 °F
perpendicular to the c-axis
Specific Heat Capacity 0.523 J/g-°C0.125 BTU/lb-°F
 0.560 J/g-°C
@Temperature 200 °C
0.134 BTU/lb-°F
@Temperature 392 °F
 0.620 J/g-°C
@Temperature 400 °C
0.148 BTU/lb-°F
@Temperature 752 °F
 0.690 J/g-°C
@Temperature 600 °C
0.165 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity 19.9 W/m-K138 BTU-in/hr-ft²-°F
 18.1 W/m-K
@Temperature 200 °C
126 BTU-in/hr-ft²-°F
@Temperature 392 °F
 18.1 W/m-K
@Temperature 400 °C
126 BTU-in/hr-ft²-°F
@Temperature 752 °F
 19.1 W/m-K
@Temperature 600 °C
133 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 21.5 W/m-K
@Temperature 800 °C
149 BTU-in/hr-ft²-°F
@Temperature 1470 °F
Melting Point <= 1660 °C<= 3020 °F
Liquidus 1660 °C3020 °F
Beta Transus 920 °C1690 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.30
@Temperature 710 °C
0.30
@Temperature 1310 °F
High purity Ti
Reflection Coefficient, Visible (0-1) 0.560.56High purity Ti; visible light.
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.10 %<= 0.10 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe <= 0.30 %<= 0.30 %
Nitrogen, N <= 0.050 %<= 0.050 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.35 %<= 0.35 %
Titanium, Ti >= 98.885 %>= 98.885 %
 
Descriptive Properties
Crystal Structurebccabove 920°C
 cphbelow 900°C

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Grade 2
Titanium Grade 4
Titanium Grade 1
Titanium Grade 7
Overview of materials for High Density Polyethylene (HDPE), Ultra High Molecular Weight

MTU030 / 14261

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.