MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Latrobe Lescalloy® 16NCD13 VAC-ARC High Strength Alloy Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Low Alloy Steel

Material Notes: 16NCD13 VAC-ARC is a premium quality low alloy, carburizing casehardenable vacuum arc remelted steel which takes its name from the French industry designation. In the carburized condition, its high case hardness is combined with desirable impact and fracture toughness characteristic in the core. Additionally, superior cleanliness makes Lescalloy 16NCD13 VAC-ARC steel ideally suited for critical aerospace gear and actuator applications.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 33.533.51" from quench end; Jominy End Quench Hardenability
 40401/2" from quenched end; Jominy End Quench Hardenability
 41.541.51/8" from quenched end; Jominy End Quench Hardenability
Tensile Strength, Ultimate 827 MPa120000 psi621°C Temper Temperature
 1100 MPa160000 psi496°C Temper Temperature
 1380 MPa200000 psi177°C Temper Temperature
Tensile Strength, Yield 931 MPa135000 psi621°C Temper Temperature
 1103 MPa160000 psi177°C Temper Temperature
 931 MPa
@Strain 0.2 %
135000 psi
@Strain 0.2 %
496°C Temper Temperature
Elongation at Break 13 %13 %in 5D; 177°C Temper Temperature
 16 %16 %in 5D; 496°C Temper Temperature
 23 %23 %in 5D; 621°C Temper Temperature
Charpy Impact 33.9 J25.0 ft-lb496°C Temper Temperature
 94.9 J70.0 ft-lb621°C Temper Temperature
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.15 %0.15 %
Chromium, Cr 1.0 %1.0 %
Iron, Fe 94.6 %94.6 %
Manganese, Mn 0.50 %0.50 %
Molybdenum, Mo 0.25 %0.25 %
Nickel, Ni 3.25 %3.25 %
Silicon, Si 0.25 %0.25 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Latrobe Lescalloy® 35NCD16 VAC-ARC High Strength Alloy Steel
ATI Allvac® 9310 UNS G93106, UNS H93100 Specialty Steel
Latrobe Lescalloy® UT-18 VAC-ARC ; 1.25 in. round High Strength Alloy Steel
ASTM A470-8 1Cr-1Mo-0.25V STEEL FORGINGS FOR TURBINE ROTORS AND SHAFTS (ASTM A470-8)
Latrobe Lescalloy® AF 1410 VIM-VAR ; 6 in High Strength Alloy Steel

NTIMK014 / 19362

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.