MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Hexcel® HexPly® 8551-7 Epoxy Matrix, AS4 Fiber
Categories: Polymer; Thermoset; Epoxy; Epoxy Cure Resin

Material Notes:

Information provided by HexCel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 2170 MPa
@Temperature 25.0 °C
315000 psi
@Temperature 77.0 °F
0°, Dry
Elongation at Yield 1.4 %1.4 %0°, Dry
Tensile Modulus 145 GPa21000 ksi0°, Dry
Flexural Yield Strength 1700 MPa
@Temperature 25.0 °C
247000 psi
@Temperature 77.0 °F
0°, Dry
Flexural Modulus 123 GPa
@Temperature 25.0 °C
17800 ksi
@Temperature 77.0 °F
0°, Dry
Compressive Yield Strength  262 MPa
@Temperature 82.0 °C
38000 psi
@Temperature 180 °F
Open hole compression, Wet
 303 MPa
@Temperature 25.0 °C
43900 psi
@Temperature 77.0 °F
After 1500 in-inlb/in impact, Dry
 303 MPa
@Temperature 25.0 °C
43900 psi
@Temperature 77.0 °F
Open hole compression, Dry
 1170 MPa
@Temperature 82.0 °C
170000 psi
@Temperature 180 °F
0°, Wet
 1240 MPa
@Temperature 121 °C
180000 psi
@Temperature 250 °F
0°, Dry
 1410 MPa
@Temperature 82.0 °C
205000 psi
@Temperature 180 °F
0°, Dry
 1590 MPa
@Temperature 25.0 °C
231000 psi
@Temperature 77.0 °F
0°, Dry
Compressive Modulus  123 GPa
@Temperature 82.0 °C
17800 ksi
@Temperature 180 °F
0°, Wet
 127 GPa
@Temperature 121 °C
18400 ksi
@Temperature 250 °F
0°, Dry
 129 GPa
@Temperature 104 °C
18700 ksi
@Temperature 219 °F
0°, Wet
 138 GPa
@Temperature 25.0 °C
20000 ksi
@Temperature 77.0 °F
0°, Dry
Shear Strength  50.3 MPa
@Temperature 121 °C
7300 psi
@Temperature 250 °F
Short Beam, Wet
 65.5 MPa
@Temperature 121 °C
9500 psi
@Temperature 250 °F
Short Beam, Dry
 82.7 MPa
@Temperature 82.0 °C
12000 psi
@Temperature 180 °F
Short Beam, Wet
 84.8 MPa
@Temperature 82.0 °C
12300 psi
@Temperature 180 °F
Short Beam, Dry
 107 MPa
@Temperature 25.0 °C
15500 psi
@Temperature 77.0 °F
Short Beam, Dry
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 93.3 °C200 °FEpoxy Matrix Limit

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Hexcel® HexPly® 8552 Epoxy Matrix, AS4 Fiber
Hexcel® HexPly® F650 Bismaleimide Resin with Fiberglass 7781 fabric reinforcement
Hexcel® HexPly® 8551-7 Epoxy Matrix, IM7 Fiber
Hexcel® HexPly® 8552 Epoxy Matrix, IM7 Fiber
Hexcel® HexPly® 8551-7 Epoxy Matrix

PHEXC047 / 98517

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.