MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LATI Lasulf G/20 PSU, 20% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polysulfone (PSU); Polysulfone, 20% Glass Fiber Reinforced

Material Notes: Polysulfone (PSU) based compound. Glass fibers. Low smoke density and low toxicity index. Very high dimensional stability

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Information provided by Lati Industria Termoplastici S.p.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.38 g/cc0.0499 lb/in³
Linear Mold Shrinkage, Flow 0.0015 - 0.0035 cm/cm0.0015 - 0.0035 in/in
Linear Mold Shrinkage, Transverse 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/in
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  55.0 MPa
@Temperature 150 °C
7980 psi
@Temperature 302 °F
 70.0 MPa
@Temperature 120 °C
10200 psi
@Temperature 248 °F
 85.0 MPa
@Temperature 90.0 °C
12300 psi
@Temperature 194 °F
 90.0 MPa
@Temperature 60.0 °C
13100 psi
@Temperature 140 °F
 100 MPa
@Temperature 23.0 °C
14500 psi
@Temperature 73.4 °F
Elongation at Break  1.8 %
@Temperature 150 °C
1.8 %
@Temperature 302 °F
 1.9 %
@Temperature 90.0 °C
1.9 %
@Temperature 194 °F
 1.9 %
@Temperature 120 °C
1.9 %
@Temperature 248 °F
 2.1 %
@Temperature 60.0 °C
2.1 %
@Temperature 140 °F
 2.3 %
@Temperature 23.0 °C
2.3 %
@Temperature 73.4 °F
Tensile Modulus  5.20 GPa
@Temperature 150 °C
754 ksi
@Temperature 302 °F
 5.50 GPa
@Temperature 120 °C
798 ksi
@Temperature 248 °F
 5.60 GPa
@Temperature 90.0 °C
812 ksi
@Temperature 194 °F
 5.80 GPa
@Temperature 60.0 °C
841 ksi
@Temperature 140 °F
 6.00 GPa
@Temperature 23.0 °C
870 ksi
@Temperature 73.4 °F
Charpy Impact Unnotched 3.00 J/cm²14.3 ft-lb/in²
Charpy Impact, Notched 0.800 J/cm²3.81 ft-lb/in²
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 125 V125 VA solution
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 160 °C320 °F
Deflection Temperature at 0.46 MPa (66 psi) 185 °C365 °F
Deflection Temperature at 1.8 MPa (264 psi) 180 °C356 °F
Vicat Softening Point 185 °C
@Load 5.00 kg
365 °F
@Load 11.0 lb
Flammability, UL94  V-1
@Thickness 1.50 mm
V-1
@Thickness 0.0591 in
 V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
Oxygen Index 38 %38 %
Glow Wire Test  960 °C
@Thickness 1.00 mm
1760 °F
@Thickness 0.0394 in
GWFI/GWT
 960 °C
@Thickness 2.00 mm
1760 °F
@Thickness 0.0787 in
GWFI/GWT
 
Processing PropertiesMetricEnglishComments
Melt Temperature 300 - 330 °C572 - 626 °F
Mold Temperature 120 - 140 °C248 - 284 °F
Drying Temperature 110 - 130 °C
@Time 10800 sec
230 - 266 °F
@Time 3.00 hour
 
Descriptive Properties
ISO Shrinkage - Pressure60 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ensinger TECATRON™ PPS Polyphenylene sulfide (PPS)
Ensinger TECATRON™ GF 40 Polyphenylene sulfide (PPS)
Vyncolit X611 Novolac Phenolic
LATI Latilub 95-15T PSU, PTFE Filled
LATI Lasulf PSU

PLATH9673 / 177369

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.