Physical Properties | Metric | English | Comments |
---|
Density | 7.61 g/cc | 0.275 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 200 | 200 |
| 110 @Temperature 870 °C | 110 @Temperature 1600 °F |
| 143 @Temperature 760 °C | 143 @Temperature 1400 °F |
| 144 @Temperature 650 °C | 144 @Temperature 1200 °F |
| 145 @Temperature 540 °C | 145 @Temperature 1000 °F |
| 148 @Temperature 425 °C | 148 @Temperature 797 °F |
| 155 @Temperature 315 °C | 155 @Temperature 599 °F |
| 168 @Temperature 205 °C | 168 @Temperature 401 °F |
| 187 @Temperature 95.0 °C | 187 @Temperature 203 °F |
Hardness, Knoop | 222 | 222 |
| 128 @Temperature 870 °C | 128 @Temperature 1600 °F |
| 163 @Temperature 760 °C | 163 @Temperature 1400 °F |
| 164 @Temperature 650 °C | 164 @Temperature 1200 °F |
| 165 @Temperature 540 °C | 165 @Temperature 1000 °F |
| 168 @Temperature 425 °C | 168 @Temperature 797 °F |
| 175 @Temperature 315 °C | 175 @Temperature 599 °F |
| 189 @Temperature 205 °C | 189 @Temperature 401 °F |
| 209 @Temperature 95.0 °C | 209 @Temperature 203 °F |
Hardness, Rockwell B | 92 | 92 |
| 63 @Temperature 870 °C | 63 @Temperature 1600 °F |
| 78 @Temperature 540 °C | 78 @Temperature 1000 °F |
| 78 @Temperature 650 °C | 78 @Temperature 1200 °F |
| 78 @Temperature 760 °C | 78 @Temperature 1400 °F |
| 79 @Temperature 425 °C | 79 @Temperature 797 °F |
| 82 @Temperature 315 °C | 82 @Temperature 599 °F |
| 85 @Temperature 205 °C | 85 @Temperature 401 °F |
| 90 @Temperature 95.0 °C | 90 @Temperature 203 °F |
Hardness, Vickers | 210 | 210 |
| 114 @Temperature 870 °C | 114 @Temperature 1600 °F |
| 149 @Temperature 760 °C | 149 @Temperature 1400 °F |
| 150 @Temperature 650 °C | 150 @Temperature 1200 °F |
| 151 @Temperature 540 °C | 151 @Temperature 1000 °F |
| 154 @Temperature 425 °C | 154 @Temperature 797 °F |
| 162 @Temperature 315 °C | 162 @Temperature 599 °F |
| 176 @Temperature 205 °C | 176 @Temperature 401 °F |
| 196 @Temperature 95.0 °C | 196 @Temperature 203 °F |
Tensile Strength, Ultimate | 734 MPa | 106000 psi |
| 754 MPa | 109000 psi |
| 208 MPa @Temperature 870 °C | 30200 psi @Temperature 1600 °F |
| 255 MPa @Temperature 815 °C | 37000 psi @Temperature 1500 °F |
| 343 MPa @Temperature 760 °C | 49700 psi @Temperature 1400 °F |
| 407 MPa @Temperature 705 °C | 59000 psi @Temperature 1300 °F |
| 459 MPa @Temperature 650 °C | 66600 psi @Temperature 1200 °F |
| 494 MPa @Temperature 595 °C | 71600 psi @Temperature 1100 °F |
| 520 MPa @Temperature 540 °C | 75400 psi @Temperature 1000 °F |
| 532 MPa @Temperature 480 °C | 77200 psi @Temperature 896 °F |
| 540 MPa @Temperature 425 °C | 78300 psi @Temperature 797 °F |
| 548 MPa @Temperature 370 °C | 79500 psi @Temperature 698 °F |
| 555 MPa @Temperature 315 °C | 80500 psi @Temperature 599 °F |
| 566 MPa @Temperature 260 °C | 82100 psi @Temperature 500 °F |
| 582 MPa @Temperature 205 °C | 84400 psi @Temperature 401 °F |
| 620 MPa @Temperature 150 °C | 89900 psi @Temperature 302 °F |
| 640 MPa @Temperature 95.0 °C | 92800 psi @Temperature 203 °F |
| 883 MPa @Temperature -18.0 °C | 128000 psi @Temperature -0.400 °F |
| 1023 MPa @Temperature -73.0 °C | 148400 psi @Temperature -99.4 °F |
| 1156 MPa @Temperature -130 °C | 167700 psi @Temperature -202 °F |
| 1405 MPa @Temperature -255 °C | 203800 psi @Temperature -427 °F |
| 1502 MPa @Temperature -195 °C | 217800 psi @Temperature -319 °F |
Tensile Strength, Yield | 390 MPa @Strain 0.2 % | 56600 psi @Strain 0.2 % |
| 401 MPa @Strain 0.2 % | 58200 psi @Strain 0.2 % |
| 113 MPa @Strain 0.2 %, Temperature 870 °C | 16400 psi @Strain 0.2 %, Temperature 1600 °F |
| 164 MPa @Strain 0.2 %, Temperature 815 °C | 23800 psi @Strain 0.2 %, Temperature 1500 °F |
| 174 MPa @Strain 0.2 %, Temperature 760 °C | 25200 psi @Strain 0.2 %, Temperature 1400 °F |
| 189 MPa @Strain 0.2 %, Temperature 705 °C | 27400 psi @Strain 0.2 %, Temperature 1300 °F |
| 193 MPa @Strain 0.2 %, Temperature 540 °C | 28000 psi @Strain 0.2 %, Temperature 1000 °F |
| 194 MPa @Strain 0.2 %, Temperature 650 °C | 28100 psi @Strain 0.2 %, Temperature 1200 °F |
| 195 MPa @Strain 0.2 %, Temperature 480 °C | 28300 psi @Strain 0.2 %, Temperature 896 °F |
| 198 MPa @Strain 0.2 %, Temperature 595 °C | 28700 psi @Strain 0.2 %, Temperature 1100 °F |
| 200 MPa @Strain 0.2 %, Temperature 425 °C | 29000 psi @Strain 0.2 %, Temperature 797 °F |
| 201 MPa @Strain 0.2 %, Temperature 370 °C | 29200 psi @Strain 0.2 %, Temperature 698 °F |
| 205 MPa @Strain 0.2 %, Temperature 315 °C | 29700 psi @Strain 0.2 %, Temperature 599 °F |
| 221 MPa @Strain 0.2 %, Temperature 260 °C | 32100 psi @Strain 0.2 %, Temperature 500 °F |
| 226 MPa @Strain 0.2 %, Temperature 205 °C | 32800 psi @Strain 0.2 %, Temperature 401 °F |
| 261 MPa @Strain 0.2 %, Temperature 150 °C | 37900 psi @Strain 0.2 %, Temperature 302 °F |
| 306 MPa @Strain 0.2 %, Temperature 95.0 °C | 44400 psi @Strain 0.2 %, Temperature 203 °F |
| 464 MPa @Strain 0.2 %, Temperature -18.0 °C | 67300 psi @Strain 0.2 %, Temperature -0.400 °F |
| 537 MPa @Strain 0.2 %, Temperature -73.0 °C | 77900 psi @Strain 0.2 %, Temperature -99.4 °F |
| 603 MPa @Strain 0.2 %, Temperature -130 °C | 87500 psi @Strain 0.2 %, Temperature -202 °F |
| 699 MPa @Strain 0.2 %, Temperature -195 °C | 101000 psi @Strain 0.2 %, Temperature -319 °F |
| 864 MPa @Strain 0.2 %, Temperature -255 °C | 125000 psi @Strain 0.2 %, Temperature -427 °F |
Elongation at Break | 61.7 % | 61.7 % |
| 66.4 % | 66.4 % |
| 23.5 % @Temperature -255 °C | 23.5 % @Temperature -427 °F |
| 41.4 % @Temperature 705 °C | 41.4 % @Temperature 1300 °F |
| 47.1 % @Temperature 760 °C | 47.1 % @Temperature 1400 °F |
| 48.2 % @Temperature 650 °C | 48.2 % @Temperature 1200 °F |
| 48.7 % @Temperature 595 °C | 48.7 % @Temperature 1100 °F |
| 52.2 % @Temperature 540 °C | 52.2 % @Temperature 1000 °F |
| 53.9 % @Temperature 480 °C | 53.9 % @Temperature 896 °F |
| 56.5 % @Temperature 425 °C | 56.5 % @Temperature 797 °F |
| 59.1 % @Temperature 370 °C | 59.1 % @Temperature 698 °F |
| 59.5 % @Temperature -195 °C | 59.5 % @Temperature -319 °F |
| 59.6 % @Temperature 315 °C | 59.6 % @Temperature 599 °F |
| 61.5 % @Temperature 260 °C | 61.5 % @Temperature 500 °F |
| 62.4 % @Temperature -130 °C | 62.4 % @Temperature -202 °F |
| 63.3 % @Temperature 95.0 °C | 63.3 % @Temperature 203 °F |
| 64 % @Temperature 205 °C | 64 % @Temperature 401 °F |
| 64.4 % @Temperature 150 °C | 64.4 % @Temperature 302 °F |
| 70.5 % @Temperature -73.0 °C | 70.5 % @Temperature -99.4 °F |
| 71.3 % @Temperature -18.0 °C | 71.3 % @Temperature -0.400 °F |
| 72.8 % @Temperature 815 °C | 72.8 % @Temperature 1500 °F |
| 72.8 % @Temperature 870 °C | 72.8 % @Temperature 1600 °F |
Modulus of Elasticity | 180 GPa | 26100 ksi |
Machinability | 23 % | 23 % |
Charpy Impact | 313 J | 231 ft-lb |
| 187 J @Temperature -195 °C | 138 ft-lb @Temperature -319 °F |
| 230 J @Temperature -130 °C | 170 ft-lb @Temperature -202 °F |
| 267 J @Temperature -73.0 °C | 197 ft-lb @Temperature -99.4 °F |
| 293 J @Temperature -18.0 °C | 216 ft-lb @Temperature -0.400 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000982 ohm-cm @Temperature 23.0 °C | 0.0000982 ohm-cm @Temperature 73.4 °F |
Magnetic Permeability | <= 1.02 | <= 1.02 |
| <= 1.02 | <= 1.02 |
| <= 1.05 | <= 1.05 |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 15.8 µm/m-°C @Temperature 25.0 - 95.0 °C | 8.78 µin/in-°F @Temperature 77.0 - 203 °F |
| 16.6 µm/m-°C @Temperature 205 °C | 9.22 µin/in-°F @Temperature 401 °F |
| 17.3 µm/m-°C @Temperature 25.0 - 315 °C | 9.61 µin/in-°F @Temperature 77.0 - 599 °F |
| 17.6 µm/m-°C @Temperature 425 °C | 9.78 µin/in-°F @Temperature 797 °F |
| 18.0 µm/m-°C @Temperature 25.0 - 540 °C | 10.0 µin/in-°F @Temperature 77.0 - 1000 °F |
| 18.5 µm/m-°C @Temperature 25.0 - 650 °C | 10.3 µin/in-°F @Temperature 77.0 - 1200 °F |
| 18.9 µm/m-°C @Temperature 25.0 - 760 °C | 10.5 µin/in-°F @Temperature 77.0 - 1400 °F |
| 19.3 µm/m-°C @Temperature 25.0 - 870 °C | 10.7 µin/in-°F @Temperature 77.0 - 1600 °F |
| 19.8 µm/m-°C @Temperature 25.0 - 980 °C | 11.0 µin/in-°F @Temperature 77.0 - 1800 °F |
Specific Heat Capacity | 0.480 J/g-°C | 0.115 BTU/lb-°F |
Thermal Conductivity | 20.7 W/m-K | 144 BTU-in/hr-ft²-°F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | <= 0.10 % | <= 0.10 % |
Chromium, Cr | 16 - 18 % | 16 - 18 % |
Iron, Fe | 59.15 - 65.42 % | 59.15 - 65.42 % |
Manganese, Mn | 7.0 - 9.0 % | 7.0 - 9.0 % |
Nickel, Ni | 8.0 - 9.0 % | 8.0 - 9.0 % |
Nitrogen, N | 0.080 - 0.18 % | 0.080 - 0.18 % |
Phosphorus, P | <= 0.040 % | <= 0.040 % |
Silicon, Si | 3.5 - 4.5 % | 3.5 - 4.5 % |
Sulfur, S | <= 0.030 % | <= 0.030 % |