Physical Properties | Metric | English | Comments |
---|
Density | 1.30 - 1.75 g/cc | 0.0470 - 0.0632 lb/in³ |
| 1.23 - 1.33 g/cc @Temperature 220 - 325 °C | 0.0444 - 0.0480 lb/in³ @Temperature 428 - 617 °F |
Filler Content | 33.0 - 44.0 % | 33.0 - 44.0 % |
Water Absorption | 0.200 - 7.10 % | 0.200 - 7.10 % |
Moisture Absorption at Equilibrium | 0.250 - 6.20 % | 0.250 - 6.20 % |
| 1.50 - 2.10 % @Temperature 70.0 - 70.0 °C | 1.50 - 2.10 % @Temperature 158 - 158 °F |
Water Absorption at Saturation | 3.50 - 7.50 % | 3.50 - 7.50 % |
Additive Loading | 40.0 % | 40.0 % |
Viscosity | 2.60 - 50.0 cP | 2.60 - 50.0 cP |
| 30.0 - 1000 cP @Temperature 240 - 280 °C | 30.0 - 1000 cP @Temperature 464 - 536 °F |
| 30.0 - 1000 cP @Shear Rate 100 - 10000 1/s | 30.0 - 1000 cP @Shear Rate 100 - 10000 1/s |
Viscosity Test | 145 - 150 cm³/g | 1.45 - 1.50 dl/g |
Viscosity Number | 100 - 150 cm³/g | 1.00 - 1.50 dl/g |
Maximum Moisture Content | 0.0200 - 0.200 | 0.0200 - 0.200 |
| 0.300 - 0.300 @Temperature 120 - 120 °C | 0.300 - 0.300 @Temperature 248 - 248 °F |
| 0.300 - 0.300 @Time 299 - 299 sec | 0.300 - 0.300 @Time 0.0830 - 0.0830 hour |
Linear Mold Shrinkage | 0.000300 - 0.0350 cm/cm | 0.000300 - 0.0350 in/in |
| 0.00200 - 0.00300 cm/cm @Temperature 80.0 - 80.0 °C | 0.00200 - 0.00300 in/in @Temperature 176 - 176 °F |
Linear Mold Shrinkage, Transverse | 0.000700 - 0.0590 cm/cm | 0.000700 - 0.0590 in/in |
| 0.00700 - 0.00700 cm/cm @Temperature 80.0 - 80.0 °C | 0.00700 - 0.00700 in/in @Temperature 176 - 176 °F |
Melt Flow | 1.00 - 78.7 g/10 min | 1.00 - 78.7 g/10 min |
Spiral Flow | 48.0 - 610 cm | 18.9 - 240 in |
Ash | 38.0 - 46.0 % | 38.0 - 46.0 % |
| 58.0 - 62.0 % @Temperature 625 - 625 °C | 58.0 - 62.0 % @Temperature 1160 - 1160 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell M | 88.0 - 108 | 88.0 - 108 |
Hardness, Rockwell R | 109 - 124 | 109 - 124 |
Hardness, Shore D | 77.0 - 84.0 | 77.0 - 84.0 |
Ball Indentation Hardness | 84.0 - 310 MPa | 12200 - 45000 psi |
Tensile Strength, Ultimate | 65.0 - 470 MPa | 9430 - 68200 psi |
| 77.0 - 281.306 MPa @Temperature -40.0 - 150 °C | 11200 - 40800.1 psi @Temperature -40.0 - 302 °F |
| 40.0 - 160 MPa @Temperature 60.0 - 150 °C | 5800 - 23200 psi @Temperature 140 - 302 °F |
| 40.0 - 160 MPa @Strain 1.00 - 3.00 % | 5800 - 23200 psi @Strain 1.00 - 3.00 % |
Tensile Strength, Yield | 74.0 - 234 MPa | 10700 - 34000 psi |
Elongation at Break | 1.00 - 11.0 % | 1.00 - 11.0 % |
| 2.60 - 7.00 % @Temperature -40.0 - 150 °C | 2.60 - 7.00 % @Temperature -40.0 - 302 °F |
Elongation at Yield | 2.00 - 9.50 % | 2.00 - 9.50 % |
Modulus of Elasticity | 4.60 - 15.9 GPa | 667 - 2300 ksi |
| 3.70 - 12.0 GPa @Temperature -40.0 - 150 °C | 537 - 1740 ksi @Temperature -40.0 - 302 °F |
Flexural Yield Strength | 97.2 - 370 MPa | 14100 - 53700 psi |
| 138 - 450 MPa @Temperature -40.0 - 121 °C | 20000 - 65300 psi @Temperature -40.0 - 250 °F |
Flexural Modulus | 1.18 - 13.8 GPa | 171 - 2000 ksi |
| 4.83 - 12.4795 GPa @Temperature -40.0 - 121 °C | 701 - 1810.03 ksi @Temperature -40.0 - 250 °F |
Flexural Strain at Break | 3.40 - 6.00 % | 3.40 - 6.00 % |
Compressive Yield Strength | 149 - 258 MPa | 21600 - 37400 psi |
Poissons Ratio | 0.330 - 0.350 | 0.330 - 0.350 |
Shear Modulus | 4.60 - 5.00 GPa | 667 - 725 ksi |
Shear Strength | 60.0 - 77.2 MPa | 8700 - 11200 psi |
Izod Impact, Notched | 0.140 - 13.2 J/cm | 0.262 - 24.8 ft-lb/in |
| 0.0800 - 5.12544 J/cm @Temperature -40.0 - 121 °C | 0.150 - 9.60205 ft-lb/in @Temperature -40.0 - 250 °F |
| 0.74746 - 1.28136 J/cm @Temperature -40.0 - -40.0 °C | 1.4003 - 2.40051 ft-lb/in @Temperature -40.0 - -40.0 °F |
| 0.74746 - 1.28136 J/cm @Thickness 3.17 - 3.17 mm | 1.4003 - 2.40051 ft-lb/in @Thickness 0.125 - 0.125 in |
Izod Impact, Unnotched | 0.770 - 14.4 J/cm | 1.44 - 27.0 ft-lb/in |
| 0.710 - 0.750 J/cm @Temperature -30.0 - -30.0 °C | 1.33 - 1.41 ft-lb/in @Temperature -22.0 - -22.0 °F |
Izod Impact, Notched (ISO) | 7.00 - 79.0 kJ/m² | 3.33 - 37.6 ft-lb/in² |
| 8.00 - 18.0 kJ/m² @Temperature -40.0 - -30.0 °C | 3.81 - 8.57 ft-lb/in² @Temperature -40.0 - -22.0 °F |
Izod Impact, Unnotched (ISO) | 24.0 - 110 kJ/m² | 11.4 - 52.3 ft-lb/in² |
| 18.0 - 95.0 kJ/m² @Temperature -30.0 - -30.0 °C | 8.57 - 45.2 ft-lb/in² @Temperature -22.0 - -22.0 °F |
Charpy Impact Unnotched | 3.50 J/cm² - NB | 16.7 ft-lb/in² - NB |
| 3.30 J/cm² - NB @Temperature -40.0 - -20.0 °C | 15.7 ft-lb/in² - NB @Temperature -40.0 - -4.00 °F |
Charpy Impact, Notched | 0.380 - 11.7 J/cm² | 1.81 - 55.4 ft-lb/in² |
| 0.370 - 11.0 J/cm² @Temperature -40.0 - -20.0 °C | 1.76 - 52.4 ft-lb/in² @Temperature -40.0 - -4.00 °F |
Puncture Energy | 2.30 - 9.10 J | 1.70 - 6.71 ft-lb |
| 1.60 - 6.00 J @Temperature -30.0 - -30.0 °C | 1.18 - 4.43 ft-lb @Temperature -22.0 - -22.0 °F |
Tensile Creep Modulus, 1 hour | 6000 - 11000 MPa | 870000 - 1.60e+6 psi |
Tensile Creep Modulus, 1000 hours | 3300 - 9500 MPa | 479000 - 1.38e+6 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 1.00e+6 - 1.00e+18 ohm-cm | 1.00e+6 - 1.00e+18 ohm-cm |
| 1.00e+8 - 1.00e+16 ohm-cm @Temperature 40.0 - 140 °C | 1.00e+8 - 1.00e+16 ohm-cm @Temperature 104 - 284 °F |
Surface Resistance | 1e+05 - 1.00e+16 ohm | 1e+05 - 1.00e+16 ohm |
Dielectric Constant | 1.50 - 15.0 | 1.50 - 15.0 |
Dielectric Strength | 7.87 - 80.0 kV/mm | 200 - 2030 kV/in |
Dissipation Factor | 0.00500 - 0.300 | 0.00500 - 0.300 |
Comparative Tracking Index | 275 - 600 V | 275 - 600 V |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 7.00 - 60.0 µm/m-°C | 3.89 - 33.3 µin/in-°F |
| 13.0 - 18.0 µm/m-°C @Temperature 55.0 - 160 °C | 7.22 - 10.0 µin/in-°F @Temperature 131 - 320 °F |
| 21.0 - 21.0 µm/m-°C @Temperature 35.0 - 55.0 °C | 11.7 - 11.7 µin/in-°F @Temperature 95.0 - 131 °F |
| 21.0 - 21.0 µm/m-°C @Thickness 2.00 - 2.00 mm | 11.7 - 11.7 µin/in-°F @Thickness 0.0787 - 0.0787 in |
CTE, linear, Transverse to Flow | 15.0 - 140 µm/m-°C | 8.33 - 77.8 µin/in-°F |
| 66.0 - 80.0 µm/m-°C @Temperature 55.0 - 160 °C | 36.7 - 44.4 µin/in-°F @Temperature 131 - 320 °F |
Specific Heat Capacity | 1.30 - 2.52 J/g-°C | 0.311 - 0.603 BTU/lb-°F |
| 1.86 - 2.10 J/g-°C @Temperature 270 - 325 °C | 0.445 - 0.502 BTU/lb-°F @Temperature 518 - 617 °F |
Thermal Conductivity | 0.280 - 0.490 W/m-K | 1.94 - 3.40 BTU-in/hr-ft²-°F |
| 0.250 - 0.280 W/m-K @Temperature 270 - 325 °C | 1.74 - 1.94 BTU-in/hr-ft²-°F @Temperature 518 - 617 °F |
Melting Point | 210 - 325 °C | 410 - 617 °F |
Maximum Service Temperature, Air | 90.0 - 270 °C | 194 - 518 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 195 - 284 °C | 383 - 543 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 102 - 280 °C | 216 - 536 °F |
Deflection Temperature at 8.0 MPa | 120 - 200 °C | 248 - 392 °F |
Vicat Softening Point | 200 - 290 °C | 392 - 554 °F |
Glass Transition Temp, Tg | 15.0 - 135 °C | 59.0 - 275 °F |
Decomposition Temperature | 300 - 350 °C | 572 - 662 °F |
UL RTI, Electrical | 120 - 140 °C | 248 - 284 °F |
UL RTI, Mechanical with Impact | 90.0 - 125 °C | 194 - 257 °F |
UL RTI, Mechanical without Impact | 130 - 150 °C | 266 - 302 °F |
Flammability, UL94 | HB - 5VB | HB - 5VB |
Flame Spread | 0.000 - 102 mm/min | 0.000 - 4.02 in/min |
Oxygen Index | 22.0 - 27.0 % | 22.0 - 27.0 % |
Glow Wire Test | 550 - 750 °C | 1020 - 1380 °F |
Ignition Temperature | 400 - 470 °C | 752 - 878 °F |
|
Processing Properties | Metric | English | Comments |
---|
Processing Temperature | 70.0 - 288 °C | 158 - 550 °F |
Nozzle Temperature | 230 - 299 °C | 446 - 570 °F |
Melt Temperature | 216 - 370 °C | 420 - 698 °F |
Mold Temperature | 26.7 - 180 °C | 80.0 - 356 °F |
Injection Velocity | 30.0 - 76.2 mm/sec | 1.18 - 3.00 in/sec |
Drying Temperature | 65.6 - 180 °C | 150 - 356 °F |
Moisture Content | 0.0300 - 0.200 % | 0.0300 - 0.200 % |
Dew Point | -28.9 - -17.8 °C | -20.0 - 0.000 °F |
Injection Pressure | 3.45 - 138 MPa | 500 - 20000 psi |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.