MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Eastman Neostar FN005 Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE; Polyester, TP

Material Notes: Neostar FN005 elastomer is a tough, clear, durable copolyester ether. It was designed for use in the profile and automotive markets, but is also used in packaging and tubing applications where toughness and flex-crack resistance are required. Neostar FN005 can be used in injection molding and cast film or tubing extrusion applications or in any application that demands strength, durability, and puncture resistance in harsh environments. This copolyester combines toughness, clarity, and flexibility without the addition of plasticizers. Neostar FN005 is considered environmentally preferred because of its non-halogenated material composition. The target inherent viscosity of this product is 1.05.

Applications/Uses

  • Automotive
  • Flexible hinges
  • Pricing channels
  • Retail pricing fins
  • Driver and passenger side air bags
  • Packaging
  • Profiles
  • Tubing
  • Key Attributes

  • Environmentally preferred, non-halogenated material
  • Excellent chemical resistance
  • Exceptional heat resistance and high temperature dimensional stability
  • High flexibility without plasticizers
  • Solvent bondable
  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Specific Gravity 1.13 g/cc1.13 g/ccASTM D792
    Water Absorption 0.35 %0.35 %24h Immersion; ASTM D570
    Viscosity Measurement 1.051.05Inherent; EMN-A-AC-G-V-1
    Melt Flow 20 g/10 min
    @Load 2.16 kg,
    Temperature 230 °C
    20 g/10 min
    @Load 4.76 lb,
    Temperature 446 °F
    ASTM D1238
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Shore A 9595ASTM D2240
    Hardness, Shore D 5555ASTM D2240
    Tensile Strength at Break 20.0 MPa2900 psiASTM D638
    Tensile Strength, Yield 14.0 MPa2030 psiASTM D638
    Elongation at Break 300 %300 %ASTM D638
    Elongation at Yield 30 %30 %ASTM D638
    Tensile Modulus 0.170 GPa24.7 ksiASTM D638
    Flexural Modulus 0.150 GPa21.8 ksiASTM D790
    Izod Impact, Notched 0.500 J/cm
    @Temperature -40.0 °C
    0.937 ft-lb/in
    @Temperature -40.0 °F
    ASTM D256
    Tear Strength, Total 370 N83.2 lb (f)ASTM D1004
     
    Thermal PropertiesMetricEnglishComments
    Heat of Fusion 27.0 J/g11.6 BTU/lbASTM E793
    CTE, linear 150 µm/m-°C
    @Temperature 20.0 °C
    83.3 µin/in-°F
    @Temperature 68.0 °F
    ASTM D696
    Specific Heat Capacity 1.60 J/g-°C0.382 BTU/lb-°FDSC
     1.80 J/g-°C
    @Temperature 100 °C
    0.430 BTU/lb-°F
    @Temperature 212 °F
    DSC
     2.00 J/g-°C
    @Temperature 150 °C
    0.478 BTU/lb-°F
    @Temperature 302 °F
    DSC
     2.30 J/g-°C
    @Temperature 175 °C
    0.550 BTU/lb-°F
    @Temperature 347 °F
    solid; DSC
     2.30 J/g-°C
    @Temperature 225 °C
    0.550 BTU/lb-°F
    @Temperature 437 °F
    melt; DSC
     3.10 J/g-°C
    @Temperature 200 °C
    0.741 BTU/lb-°F
    @Temperature 392 °F
    transition; DSC
    Thermal Conductivity 0.190 W/m-K1.32 BTU-in/hr-ft²-°FASTM C177
    Melting Point 207 °C405 °FCrystalline Peak; ASTM D3418
    Crystallization Temperature 140 °C284 °Fon cooling; DSC
    Vicat Softening Point 170 °C338 °F1kg load; ASTM D1525
    Brittleness Temperature <= -75.0 °C<= -103 °FASTM D746
    Glass Transition Temp, Tg -3.00 °C26.6 °FDSC
    Clash Berg Stiffness Temperature <= -70.0 °C<= -94.0 °Fat 930 MPa; ASTM D1043
     -28.0 °C-18.4 °Fat 240 MPa; ASTM D1043

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Eastman Neostar FN007 Elastomer
    Celanese Riteflex® 647 Thermoplastic Polyester Elastomer (TPE)
    Eastman AP006 Copolyester
    Eastman Neostar FN006 Elastomer
    Envalior Arnitel® EL550 Polyether Ester Elastomer (European and Asian Grade)

    PE9089 / 35145

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.