MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Chemours 350 PFA Perfluoroalkoxy Copolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA)

Material Notes: Combines the processing ease of conventional thermoplastic resins with the excellent properties of PTFE. High chemical resistance, superior electrical properties, high service temperatures, superior high temperature creep resistance, excellent low temperature toughness, and exceptional flame resistance. Processed by conventional melt-extrusion and molding techniques. Resin Characteristics: Premium resin with enhanced ESCR. Lowest flow rate of this series. Uses: Films; chemical linings; transfer-molded articles; tubing.

Chemours was formed from former DuPont performance chemicals businesses, including DuPont Fluoroproducts, in 2015. This specific product was discontinued prior to the formation of Chemours.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.12 - 2.17 g/cc2.12 - 2.17 g/ccASTM D792
Water Absorption <= 0.030 %<= 0.030 %24 hours; ASTM D570
Melt Flow 2.0 g/10 min2.0 g/10 minASTM D3307
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5555ASTM D2240
Tensile Strength, Ultimate 28.0 MPa4060 psiASTM D3307
 14.0 MPa
@Temperature 250 °C
2030 psi
@Temperature 482 °F
ASTM D3307
 129 MPa
@Temperature -196 °C
18700 psi
@Temperature -321 °F
ASTM D1780
Tensile Strength, Yield 15.2 MPa2200 psiASTM D3307
Elongation at Break 300 %300 %ASTM D3307
 8.0 %
@Temperature -196 °C
8.0 %
@Temperature -321 °F
ASTM D1708
 500 %
@Temperature 250 °C
500 %
@Temperature 482 °F
ASTM D3307
Flexural Modulus 0.625 GPa90.6 ksiASTM D790
 0.0690 GPa
@Temperature 250 °C
10.0 ksi
@Temperature 482 °F
ASTM D790
Compressive Strength  24.0 MPa
@Temperature 23.0 °C
3480 psi
@Temperature 73.4 °F
ASTM D695
 414 MPa
@Temperature -196 °C
60000 psi
@Temperature -321 °F
ASTM D695
Compressive Modulus  69.0 GPa
@Temperature 23.0 °C
10000 ksi
@Temperature 73.4 °F
ASTM D695
 4690 GPa
@Temperature -196 °C
680000 ksi
@Temperature -321 °F
ASTM D695
Izod Impact, Notched NBNBASTM D256
 0.640 J/cm
@Temperature -196 °C
1.20 ft-lb/in
@Temperature -321 °F
ASTM D256-72a
Coefficient of Friction, Dynamic 0.210.213 ft/min; 100 psi; dry vs. steel
 0.2140.21410 ft/min; 100 psi; dry vs. steel
 0.2290.22930 ft/min; 100 psi; dry vs. steel
 0.2890.28950 ft/min; 100 psi; dry vs. steel
K (wear) Factor 1400 x 10-8 mm³/N-M694 x 10-10 in³-min/ft-lb-hr50 ft/min; 100 psi; dry vs. steel
 1980 x 10-8 mm³/N-M983 x 10-10 in³-min/ft-lb-hr30 ft/min; 100 psi; dry vs. steel
 3205 x 10-8 mm³/N-M1591 x 10-10 in³-min/ft-lb-hr3 ft/min; 100 psi; dry vs. steel
 3700 x 10-8 mm³/N-M1837 x 10-10 in³-min/ft-lb-hr10 ft/min; 100 psi; dry vs. steel
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+18 ohm-cm1.00e+18 ohm-cmASTM D257
Surface Resistivity per Square >= 1.00e+17 ohm>= 1.00e+17 ohmASTM D257
Dielectric Constant 2.03
@Frequency 60.0 - 1.00e+6 Hz
2.03
@Frequency 60.0 - 1.00e+6 Hz
ASTM D150
Dielectric Strength 80.0 kV/mm
@Thickness 0.0250 mm
2030 kV/in
@Thickness 0.000984 in
Short time; ASTM D149
Dissipation Factor 0.00010
@Frequency 60.0 - 1.00e+6 Hz
0.00010
@Frequency 60.0 - 1.00e+6 Hz
ASTM D150
Arc Resistance >= 180 sec>= 180 secASTM D495
 
Thermal PropertiesMetricEnglishComments
CTE, linear  140 µm/m-°C
@Temperature 21.0 - 100 °C
77.8 µin/in-°F
@Temperature 69.8 - 212 °F
ASTM D696
 180 µm/m-°C
@Temperature 100 - 149 °C
100 µin/in-°F
@Temperature 212 - 300 °F
ASTM D696
 220 µm/m-°C
@Temperature 149 - 208 °C
122 µin/in-°F
@Temperature 300 - 406 °F
ASTMD 696
Specific Heat Capacity 1.172 J/g-°C
@Temperature 100 °C
0.2801 BTU/lb-°F
@Temperature 212 °F
Melting Point 302 - 310 °C576 - 590 °FASTM D3418
Maximum Service Temperature, Air 260 °C500 °F
Glass Transition Temp, Tg -80.0 °C-112 °FGlass II
 90.0 °C194 °FGlass I
Flammability, UL94 V-0V-0
Oxygen Index >= 95 %>= 95 %ASTM D2863
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.351.35ASTM D542-50
Haze 4.0 %4.0 %ASTM D1003-52
Transmission, Visible 91 - 96 %
@Thickness 0.0250 mm
91 - 96 %
@Thickness 0.000984 in
0.40 to 0.70 µm
IR Transmittance 96 - 98 %96 - 98 %2.5%; 0.70 to 2.40 µm
UV Transmittance 77 - 91 %
@Thickness 0.0250 mm
77 - 91 %
@Thickness 0.000984 in
0.25 to 0.70 µm
 
Processing PropertiesMetricEnglishComments
Processing Temperature 379 - 399 °C714 - 750 °FCure Temperature
 
Descriptive Properties
20% Hydrochloric Acid Transmission, g/100sq in.<0.02
50% Sodium Hydroxide Transmission, g/100sq in.<.02
Acetic Acid Transmission, g/100sq in.0.41
Acetone Transmission, g/100sq in.0.95
Acetophenone Transmission, g/100sq in.0.5
Benzene Transmission, g/100sq in.0.64
Carbon Tetrachloride Transmission, g/100sq in.0.31
Chemical/Solvent ResistanceExcellent
Ethyl Acetate Transmission, g/100sq in.0.76
Folding Endurance, # cycles, .18-.20 mm500000
Heat of Combustion J/g5300ASTM D240
Hexane Transmission, g/100sq in.0.56
Piperidine Transmission, g/100sq in.0.04
Red Fuming Nitric Acid Transmission, g/100sq in.7.5-1.4
Salt Spray Resistance on aluminum, Hours1000
Sulfuric Acid Transmission, g/100sq in.0.00001
Water Transmission, g/100sq in.0.4
Weather Resistance10Years unaffected in Florida Exposure

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chemours 340 PFA Perfluoroalkoxy Copolymer
Chemours Teflon® PFA Grade 450 HP Extrusion and Molding Resin
Quadrant Symalit® PFA Tetrafluoroethylene-perfluoroalkylvinylether (ASTM Product Data Sheet)
Chemours 100 FEP Fluorinated Ethylene Propylene
Chemours Teflon® PFA Grade 345 Extrusion and Molding Resin

PDU922 / 33333

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.