MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Meldin Supplier

DuPont Mobility and Materials Vespel® SCP-50094 Polyimide
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: Designed for those demanding applications that require even more toughness, thermal stability and chemical resistance. SCP-50094 has been put to the test in ultra-high-stress environments like aircraft engines. So, it’s ready for just about any design challenge.

Applications:

Information provided by DuPont

Information provided by DuPont. This product line has remained with DuPont after the DuPont-Dow merger.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.44 g/cc1.44 g/ccASTM D792
Water Absorption at Saturation 0.96 %0.96 %24 hours. (Weight Change); ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell E 7070ASTM D785
Tensile Strength, Ultimate 88.3 MPa12800 psi23°C (73°F); ASTM D638
 45.5 MPa
@Temperature 260 °C
6600 psi
@Temperature 500 °F
ASTM D638
Elongation at Break 2.1 %2.1 %23°C (73°F); ASTM D638
 4.6 %
@Temperature 260 °C
4.6 %
@Temperature 500 °F
ASTM D638
Modulus of Elasticity 6.49 GPa941 ksi23°C (73°F); ASTM D638
 3.72 GPa
@Temperature 260 °C
539 ksi
@Temperature 500 °F
ASTM D638
Flexural Strength 68.9 MPa10000 psi500°F; ASTM D790
 110 MPa16000 psi73°F; ASTM D790
Flexural Modulus 2.70 GPa392 ksi500°F; ASTM D790
 5.17 GPa750 ksi73°F; ASTM D790
Compressive Strain at Break  18 %
@Temperature 23.0 °C
18 %
@Temperature 73.4 °F
ASTM D695
 31 %
@Temperature 260 °C
31 %
@Temperature 500 °F
ASTM D695
Compressive Strength 64.1 MPa9300 psi@10% strain; 260°C (500°F).; ASTM D695
 77.2 MPa11200 psi260°C (500°F).; ASTM D695
 165 MPa24000 psi@10% strain; 23°C (73°F).; ASTM D695
 170 MPa24700 psi23°C (73°F).; ASTM D695
Poissons Ratio 0.250.2523°C (73°F); ASTM D638
 0.32
@Temperature 190 °C
0.32
@Temperature 374 °F
ASTM D638
Coefficient of Friction, Dynamic 0.0600.060(P=250 psi), V=400 f/m)
 0.250.25(P=187 psi); V=134 f/m)
K Factor (Wear Factor) 8.08.0Falex; (100 KPV)(3.5 MPa m/s)
 13.113.1Falex; (25 KPV)(0.875 MPa m/s)
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 59.4 µm/m-°C
@Temperature 23.0 - 300 °C
33.0 µin/in-°F
@Temperature 73.4 - 572 °F
ASTM E-831
CTE, linear, Transverse to Flow 34.2 µm/m-°C
@Temperature 23.0 - 300 °C
19.0 µin/in-°F
@Temperature 73.4 - 572 °F
ASTM E-831
Thermal Conductivity 0.392 W/m-K2.72 BTU-in/hr-ft²-°F100°C (212°F)
 0.4069 W/m-K
@Temperature 200 °C
2.820 BTU-in/hr-ft²-°F
@Temperature 392 °F
 0.4293 W/m-K
@Temperature 300 °C
2.974 BTU-in/hr-ft²-°F
@Temperature 572 °F
 
Descriptive Properties
Creep, %0.025Compressive. 23°C (73°F) 10 MPa (1.5 ksi). 10 hours
 0.04Compressive. 23°C (73°F) 10 MPa (1.5 ksi). 100 hours
PV Limit, ksi-fpm500
Thermal Oxidative Stability, %3.3371°C (700°F). 100 hours @ 70 psia; circulating air.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
DuPont Mobility and Materials VESPEL TP-8054 Polyimide
DuPont Mobility and Materials Vespel® SMP-40025 DF Polyimide
DuPont Mobility and Materials Vespel® SP-1 ISO Polyimide
DuPont Mobility and Materials Vespel® CP-0644 Polyimide
DuPont Mobility and Materials VESPEL TP-8929 Polyimide

PDU2010 / 32872

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.