MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil Optema® TC-110 Molding Ethylene Methyl Acrylate
Categories: Polymer; Thermoplastic; Ethylene Methyl Acrylate; Ethylene-Methyl Acrylate Copolymer, Compounding Grade

Material Notes: Product Description: Optema TC 110 is an ethylene methyl acrylate copolymer. TC 110 can be used for injection molding applications. It can be used in alloys, blends or compounds to increase impact strength or to lower the modulus. TC 110 can be injection molded and extruded.

Availability: Latin America, North America and South America

Additive:

  • Thermal Stabilizer: Yes
Applications:
  • Compatibilizer
  • Engineering thermoplastic impact modifier
  • Foams
  • Injection Molding
  • Soft, molded parts

Data provided by the manufacturer, Exxon Chemical.

Key Words: EMA; Exxon Chemical Company
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.942 g/cc0.0340 lb/in³Exxon Method
Methyl Acrylate Content 21.5 %21.5 %Exxon Method
Melt Flow 2.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
Exxon Method
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 86
@Time 15.0 sec
86
@Time 0.00417 hour
ASTM D2240
Hardness, Shore D 26
@Time 15.0 sec
26
@Time 0.00417 hour
ASTM D2240
Tensile Strength at Break 8.27 MPa1200 psiASTM D638
Elongation at Break >= 800 %>= 800 %ASTM D638
Flexural Modulus, 1% Secant 37.2 MPa5400 psiASTM D790
Dart Drop, Total Energy  17.6 J
@Temperature 22.8 °C
13.0 ft-lb
@Temperature 73.0 °F
ASTM D3763
 32.5 J
@Temperature -40.0 °C
24.0 ft-lb
@Temperature -40.0 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
Melting Point 77.8 °C172 °FExxon Method
Vicat Softening Point 51.1 °C124 °FPeak Melting Temperature; ASTM D1525

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil OPTEMA™ TC 120 Molding Ethylene Methyl Acrylate
ExxonMobil Optema® TC-110 Blown Ethylene Methyl Acrylate
ExxonMobil Optema® TC-110 Cast Ethylene Methyl Acrylate
ExxonMobil Optema® TC-114 Blown Ethylene Methyl Acrylate
ExxonMobil Optema® TC-114 Cast Ethylene Methyl Acrylate

PEXCEVa / 140962

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.