MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese ZENITE 6130 LCP, 30% Glass Reinforced
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), 30% Glass Fiber Filled

Material Notes: Zenite« 6130 is a 30% glass fiber reinforced liquid crystal polymer for injection molding. It has excellent impact resistance and excellent heat deflection temperature.

Information provided by Celanese Corporation.

Key Words: 30% glass reinforced
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.62 g/cc0.0585 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0015 cm/cm0.0015 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 130 MPa18900 psi5mm/min; ISO 527-2/1A
Elongation at Break 2.0 %2.0 %5mm/min; ISO 527-2/1A
Tensile Modulus 13.0 GPa1890 ksi1mm/min; ISO 527-2/1A
Flexural Strength 190 MPa27600 psiISO 178
Flexural Modulus 11.0 GPa1600 ksiISO 178
Compressive Strength 113 MPa16400 psiISO 604
Charpy Impact Unnotched 4.00 J/cm²19.0 ft-lb/in²ISO 179/1eU
 3.00 J/cm²
@Temperature -30.0 °C
14.3 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 3.50 J/cm²16.7 ft-lb/in²ISO 179/1eA
 3.00 J/cm²
@Temperature -30.0 °C
14.3 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+13 ohm-cm>= 1.00e+13 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  4.0
@Frequency 1e+6 Hz
4.0
@Frequency 1e+6 Hz
IEC 60250
 4.5
@Frequency 100 Hz
4.5
@Frequency 100 Hz
IEC 60250
Dielectric Strength 36.0 kV/mm914 kV/inIEC 60243-1
Dissipation Factor  0.015
@Frequency 100 Hz
0.015
@Frequency 100 Hz
IEC 60250
 0.031
@Frequency 1e+6 Hz
0.031
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 175 V175 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 3.00 µm/m-°C1.67 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 70.0 µm/m-°C38.9 µin/in-°FISO 11359-2
Melting Point 335 °C635 °FISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 300 °C572 °FISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 268 °C514 °FISO 75-1, -2
Glass Transition Temp, Tg 120 °C248 °FISO 11357-1,-2,-3
Flammability, UL94  V-0
@Thickness 0.200 mm
V-0
@Thickness 0.00787 in
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
Oxygen Index 41 %41 %ISO 4589
 
Processing PropertiesMetricEnglishComments
Processing Temperature 40.0 - 150 °C104 - 302 °Fcavity
Melt Temperature 350 - 360 °C662 - 680 °F
Drying Temperature 150 °C302 °F
Dry Time 3 hour3 hour
Moisture Content 0.010 %0.010 %Necessary low maximum

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese VECTRA C130 LCP, 30% Glass Reinforced
Celanese ZENITE 7130 LCP, 30% Glass Reinforced
Avient Synprene® ST-6130 Thermoplastic Elastomer - SBC
Celanese ZENITE 6130L LCP, 30% Glass Reinforced
Celanese ZENITE 5130L LCP, 30% Glass Reinforced

PHCS502 / 123917

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.