MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Akro-Plastic Akrotek® PK-VM TM (4954) PK Dry
Categories: Polymer; Thermoplastic; Polyketone

Material Notes: The renaissance of this polymer came about in 2004 with an environmental program aimed at reducing greenhouse gases. The comonomer is CO (carbon monoxide), an industrial „waste” gas, which forms an unusual product when bonding with the polymer. The terpolymer, which forms the basis of most AKROTEK® PK formulations when using the monomers ethylene and propylene, currently has the greatest significance. AKRO-PLASTIC GmbH produces two product families from this base polymer (HM = normal flow and VM = very easy-flowing), based on the former portfolio of the Shell AG, from non-reinforced to high-glass-fiber-reinforced standards, from flame-retardant to carbon-fibre-reinforced custom grades

The outstanding characteristic properties of these properties include:

  • excellent dynamic resilience
  • good barrier properties
  • good tribological properties
  • phenomenal resistance to chemicals
  • good hydrolysis resistance
  • shorter cycle times
Application areas:
  • Industry
  • Automotive industry
  • Electronics/Electrical

Information provided by Akro-Plastic GmbH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.013 cm/cm0.013 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.016 cm/cm0.016 in/inISO 294-4
Spiral Flow 120 cm47.2 inCross section: 7 mm x 3.5 mm
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 50.0 MPa7250 psi50 [mm/min]; ISO 527-2
 10.0 MPa
@Temperature 80.0 °C
1450 psi
@Temperature 176 °F
6 months in Dimethyl formamide
 13.5 MPa
@Temperature 80.0 °C
1960 psi
@Temperature 176 °F
6 months in Tetrachloroethylene
 14.0 MPa
@Temperature 80.0 °C
2030 psi
@Temperature 176 °F
3 months in Sulfuric acid 40%
 15.0 MPa
@Temperature 80.0 °C
2180 psi
@Temperature 176 °F
6 months in Acetic acid 5%
 15.0 MPa
@Temperature 80.0 °C
2180 psi
@Temperature 176 °F
3 months in Sulfuric acid 5%
 34.0 MPa
@Temperature 23.0 °C
4930 psi
@Temperature 73.4 °F
12 months in Ammonium hydroxide 10%
 42.5 MPa
@Temperature 23.0 °C
6160 psi
@Temperature 73.4 °F
12 months in Dichloroethane
 44.5 MPa
@Temperature 23.0 °C
6450 psi
@Temperature 73.4 °F
12 months in Gasohol M-85 (unleaded, 15% methanol)
 44.5 MPa
@Temperature 23.0 °C
6450 psi
@Temperature 73.4 °F
12 months in Methanol
 45.0 MPa
@Temperature 23.0 °C
6530 psi
@Temperature 73.4 °F
12 months in Dimethyl formamide
 46.0 MPa
@Temperature 45.0 °C
6670 psi
@Temperature 113 °F
12 months in Gasohol (unleaded, 10% methanol)
 46.0 MPa
@Temperature 23.0 °C
6670 psi
@Temperature 73.4 °F
12 months in Ethanol 95%
 46.0 MPa
@Temperature 23.0 °C
6670 psi
@Temperature 73.4 °F
12 months in Tetrachloroethylene
 47.0 MPa
@Temperature 23.0 °C
6820 psi
@Temperature 73.4 °F
12 months in Gasohol (unleaded, 10% methanol)
 47.5 MPa
@Temperature 23.0 °C
6890 psi
@Temperature 73.4 °F
1 month in Methanol
 48.0 MPa
@Temperature 23.0 °C
6960 psi
@Temperature 73.4 °F
12 months in Zinc chloride 10%
 48.0 MPa
@Temperature 23.0 °C
6960 psi
@Temperature 73.4 °F
6 months in Methylethylketone
 53.0 MPa
@Temperature 120 °C
7690 psi
@Temperature 248 °F
6 months in Motor oil 10W-40
 53.0 MPa
@Temperature 80.0 °C
7690 psi
@Temperature 176 °F
6 months in Sodium hypochlorite 4.6%
 54.0 MPa
@Temperature 45.0 °C
7830 psi
@Temperature 113 °F
12 months in Antifreeze 50%, water 50%
 54.9 MPa
@Temperature 45.0 °C
7960 psi
@Temperature 113 °F
12 months Automatic transmission fluid
 55.0 MPa
@Temperature 120 °C
7980 psi
@Temperature 248 °F
6 months in Brake fluid
 55.0 MPa
@Temperature 120 °C
7980 psi
@Temperature 248 °F
3 months in Antifreeze 100% ethylene glycol
 55.0 MPa
@Temperature 80.0 °C
7980 psi
@Temperature 176 °F
12 months in Butyl acetate
 55.0 MPa
@Temperature 80.0 °C
7980 psi
@Temperature 176 °F
12 months in Toluene
 55.5 MPa
@Temperature 45.0 °C
8050 psi
@Temperature 113 °F
12 months in Hydraulic fluid
 57.0 MPa
@Temperature 80.0 °C
8270 psi
@Temperature 176 °F
3 months in Sodium hydroxide 1%
 57.5 MPa
@Temperature 80.0 °C
8340 psi
@Temperature 176 °F
6 months in Ammonium hydroxide 10%
 60.5 MPa
@Temperature 80.0 °C
8770 psi
@Temperature 176 °F
12 months in Heptane
 60.5 MPa
@Temperature 80.0 °C
8770 psi
@Temperature 176 °F
6 months in Sodium chloride 10%
Elongation at Break >= 40 %>= 40 %50 [mm/min]; ISO 527-2
Tensile Modulus 1.50 GPa218 ksi1 [mm/min]; ISO 527-2
Flexural Strength 55.0 MPa7980 psi2 [mm/min]; ISO 178
Flexural Modulus 1.50 GPa218 ksi2 [mm/min]; ISO 178
Charpy Impact Unnotched  0.300 J/cm²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 10.0 J/cm²
@Temperature 23.0 °C
47.6 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
Coefficient of Friction, Dynamic 0.330.33
K (wear) Factor 0.800 x 10-8 mm³/N-M0.397 x 10-10 in³-min/ft-lb-hr
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FDIN EN 11357-1
Deflection Temperature at 0.46 MPa (66 psi) 185 °C365 °FHDT/B; ISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °C167 °FHDT/A; ISO 75-2
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
Glow Wire Flammability Index 650 °C
@Thickness 2.00 mm
1200 °F
@Thickness 0.0787 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Nozzle Temperature 230 - 250 °C446 - 482 °F
Zone 1 210 - 250 °C410 - 482 °F
Zone 2 210 - 250 °C410 - 482 °F
Zone 3 210 - 250 °C410 - 482 °F
Zone 4 210 - 250 °C410 - 482 °F
Melt Temperature 230 - 250 °C446 - 482 °F
Mold Temperature 60.0 - 80.0 °C140 - 176 °F
Drying Temperature 60.0 - 80.0 °C140 - 176 °F
Dry Time <= 4.00 hour<= 4.00 hour
Back Pressure 30.0 - 80.0 MPa4350 - 11600 psi
 
Descriptive Properties
Resistance to Acetic Acid1% Change in Volume5% Conc., 12 months at 23°C
 1% Change in Volume5% Conc., 6 months at 80°C
 3% Change in Weight5% Conc., 12 months at 23°C
 3% Change in Weight5% Conc., 6 months at 80°C
Resistance to Acetone2% Change in Volume12 months at 23°C
 5% Change in Volume12 months at 80°C
 5% Change in Weight12 months at 80°C
 5% Change in Weight12 months at 23°C
Resistance to Ammonium hydroxide 10%0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
 -3% Change in Volume6 months at 80°C
 -5% Change in Weight6 months at 80°C
Resistance to Antifreeze 50%, 50% water0% Change in Volume24 months at 23°C
 0% Change in Weight24 months at 23°C
 1% Change in Volume12 months at 45°C
 1% Change in Weight12 months at 45°C
Resistance to Antifreeze, 100% ethylene glycol0% Change in Volume24 months at 23°C
 0% Change in Weight24 months at 23°C
 5% Change in Volume3 months at 120°C
 5% Change in Weight3 months at 120°C
Resistance to Automatic transmission fluid0% Change in Volume24 months at 23°C
 0% Change in Volume12 months at 45°C
 0% Change in Weight24 months at 23°C
 0% Change in Weight12 months at 45°C
Resistance to Brake fluid0% Change in Volume24 months at 23°C
 0% Change in Weight24 months at 23°C
 5% Change in Volume6 months at 120°C
 5% Change in Weight6 months at 120°C
Resistance to Butyl acetate0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
 2% Change in Volume12 months at 80°C
 2% Change in Weight12 months at 80°C
Resistance to Calcium Chloride0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
Resistance to Chassis lube0% Change in Volume24 months at 23°C
 0% Change in Weight24 months at 23°C
 -1% Change in Volume6 months at 120°C
 -1% Change in Weight6 months at 120°C
Resistance to Dichloroethane0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
Resistance to Dimethyl formamide0% Change in Volume12 months at 23°C
 2% Change in Weight12 months at 23°C
 Samples swell and slowly dissolve6 months at 80°C, change in weight
 Samples swell and slowly dissolve6 months at 80°C, change in volume
Resistance to Ethanol1% Change in Volume95% Conc., 12 months at 23°C
 2% Change in Volume95% Conc., 12 months at 65°C
 2% Change in Weight95% Conc., 12 months at 23°C
 2% Change in Weight95% Conc., 12 months at 65°C
Resistance to Gasohol (unleaded, 10% methanol)0% Change in Volume12 months at 23°C
 1% Change in Weight12 months at 23°C
 3% Change in Weight12 months at 45°C
 5% Change in Volume12 months at 45°C
Resistance to Gasohol M-25 (unleaded, 15% methanol)0% Change in Volume1 month at 23°C
 1% Change in Weight1 month at 23°C
 3% Change in Volume12 months at 23°C
 5% Change in Weight12 months at 23°C
Resistance to Heptane0% Change in Volume12 months at 80°C
 0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
 0% Change in Weight12 months at 80°C
Resistance to Hydraulic fluid0% Change in Volume24 months at 23°C
 0% Change in Volume12 months at 45°C
 0% Change in Weight24 months at 23°C
 0% Change in Weight12 months at 45°C
Resistance to Hydrochloric acid0% change in volume10% Conc., 1 months at 80°C
 0% change in volume10% Conc., 12 months at 23°C
 2% change in weight10% Conc., 1 months at 80°C
 2% change in weight10% Conc., 12 months at 23°C
Resistance to Jet fuel A0% Change in Volume24 months at 23°C
 0% Change in Weight24 months at 23°C
 1% Change in Weight12 months at 45°C
 2% Change in Volume12 months at 45°C
Resistance to Methanol1% Change in Volume1 month
 2% Change in Weight12 months
 2% Change in Weight1 month
 3% Change in Volume12 months
Resistance to Methylethylketone2% Change in Volume6 months at 23°C
 2% Change in Weight6 months at 23°C
Resistance to Motor oil (SAE 10W-40)0% Change in Volume24 months at 23°C
 0% Change in Weight24 months at 23°C
 0% Change in Weight6 months at 120°C
 -1% Change in Volume6 months at 120°C
Resistance to MTBE1% Change in Volume12 months at 23°C
 1% Change in Weight12 months at 23°C
Resistance to Sodium Chloride 10%0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
 0% Change in Weight6 months at 80°C
 -1% Change in Volume6 months at 80°C
Resistance to Sodium hydroxide 10%0% Change in Volume12 months at 23°C
 1% Change in Weight12 months at 23°C
 5% Change in Volume3 months at 80°C
 5% Change in Weight3 months at 80°C
Resistance to Sodium hypochlorite 4.6%-1% Change in Volume6 months at 80°C
 -1% Change in Volume12 months at 23°C
 -1% Change in Weight12 months at 23°C
 -2% Change in Weight6 months at 80°C
Resistance to Sulfuric acid0% change in volume40% Conc., 12 months at 23°C
 0% change in volume5% Conc., 12 months at 23°C
 0% change in weight40% Conc., 12 months at 23°C
 -1% change in volume5% Conc., 3 months at 80°C
 -1% change in volume40% Conc., 3 months at 80°C
 1% change in weight5% Conc., 12 months at 23°C
 -1% change in weight5% Conc., 3 months at 80°C
 -1% change in weight40% Conc., 3 months at 80°C
Resistance to Tetrachloroethylene0% Change in Volume12 months at 23°C
 1% Change in Weight12 months at 23°C
 2% Change in Volume6 months at 80°C
 3% Change in Weight6 months at 80°C
Resistance to Toluene0% Change in Volume12 months at 23°C
 1% Change in Volume12 months at 80°C
 1% Change in Weight12 months at 23°C
 4% Change in Weight12 months at 80°C
Resistance to Trichlorethane0% Change in Volume12 months at 23°C
 1% Change in Volume12 months at 80°C
 1% Change in Weight12 months at 23°C
 5% Change in Weight12 months at 80°C
Resistance to Unleaded gasoline0% Change in Volume12 months at 23°C
 0% Change in Weight12 months at 23°C
 1% Change in Weight12 months at 45°C
 3% Change in Volume12 months at 45°C
Resistance to Xylene0% Change in Volume6 months at 23°C
 0% Change in Weight6 months at 23°C
Resistance to Zinc chloride 10%2% Change in Weight12 months at 23°C
 3% Change in Volume12 months at 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Akro-Plastic Akrotek® PK-HM (4773) PK Conditioned
Akro-Plastic Akrotek® PK-HM (4773) PK Dry
BASF Ultramid® A4H PA66 (Dry)
Akro-Plastic Akrotek® PK-VM (4774) PK Dry
Akro-Plastic Akrotek® PK-VM (4774) PK Conditioned

PAKRO151 / 182738

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.