MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Microtherm Group Aeroguard® SD Filament Reinforced Silica Thermal Insulation Panel, Flexible
Categories: Ceramic; Oxide; Silicon Oxide; Other Engineering Material

Material Notes: Aeroguard® is a Microtherm® Flexible Insulation Panel made under the most stringent quality control with full traceability for aerospace applications.
    Properties
  • Opacified blend of filament reinforced silica
  • Flexible Aerospace quality high temperature microporous insulation
  • Lowest thermal conductivity
  • Stable performance for continuous exposure to 1000 °C (1832 °F)
  • Non combustible. Aeroguard® HD can withstand direct fire exposure without damage
  • Easy to manipulate and shape
  • Environmentally friendly.
    Applications
  • Aircraft
  • Missiles
  • Intelligent armaments

Information provided by Microtherm.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.128 - 0.220 g/cc0.00462 - 0.00795 lb/in³dependent on panel grade, area and thickness
Thickness 3000 - 13000 microns118 - 512 mil
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity  0.680 J/g-°C
@Temperature 0.000 °C
0.163 BTU/lb-°F
@Temperature 32.0 °F
 0.920 J/g-°C
@Temperature 200 °C
0.220 BTU/lb-°F
@Temperature 392 °F
 1.00 J/g-°C
@Temperature 400 °C
0.239 BTU/lb-°F
@Temperature 752 °F
Thermal Conductivity  0.0251 W/m-K
@Temperature 100 °C
0.174 BTU-in/hr-ft²-°F
@Temperature 212 °F
@ 200 kg/m³
 0.0278 W/m-K
@Temperature 200 °C
0.193 BTU-in/hr-ft²-°F
@Temperature 392 °F
@ 200 kg/m³
 0.0310 W/m-K
@Temperature 300 °C
0.215 BTU-in/hr-ft²-°F
@Temperature 572 °F
@ 200 kg/m³
 0.0349 W/m-K
@Temperature 400 °C
0.242 BTU-in/hr-ft²-°F
@Temperature 752 °F
@ 200 kg/m³
Maximum Service Temperature, Air 500 °C932 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elektro-Isola G-Etronax EP FR4 Epoxy, Glass Fabric Reinforcement, Light Yellow, Sheets
Microtherm Group Hydrophoblic Quilted Panel Filament Reinforced Silica Thermal Insulation Panel, Flexible and Waterproof
Overview of materials for Methacrylate Adhesive
Polymer Resources PPX-FR4 Modified-PPO, V-1 Flame Retardant
SCG Chemicals EL-Lene™ H5814J High Density Polyethylene Injection Molding

CMICRO02 / 90044

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.