MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI E4340 H Steel, oil quenched 800°C (1470°F), 595°C (1100°F) temper, 25 mm round
Categories: Metal; Ferrous Metal; Alloy Steel; AISI 4000 Series Steel; Low Alloy Steel; Carbon Steel; Medium Carbon Steel

Material Notes: 57 HRC surface, 57 HRC 1/2 radius, 56 HRC center

AISI E4340H has a favorable response to heat treatment (usually oil quenching followed by tempering) and exhibits a good combination of ductility and strength when treated thusly. Uses include piston pins, bearings, ordnance, gears, dies, and pressure vessels.

Key Words: AISI E4340H; alloy steels, UNS H43406, ASTM A304, SAE J1268, DIN 1.6562
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.85 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 331331
Hardness, Knoop 359359Converted from Brinell
Hardness, Rockwell B 9999Converted from Brinell
Hardness, Rockwell C 3636Converted from Brinell
Hardness, Vickers 350350Converted from Brinell
Tensile Strength, Ultimate 1138 MPa165100 psi
Tensile Strength, Yield 1096 MPa159000 psi
Elongation at Break 16.5 %16.5 %in 50 mm
Reduction of Area 54.1 %54.1 %
Modulus of Elasticity 200 GPa29000 ksiAISI 4340
Bulk Modulus 159 GPa23100 ksiEstimated from elastic modulus
Poissons Ratio 0.290.29Typical for steel
Machinability 50 %50 %annealed and cold drawn. Based on 100% machinability for AISI 1212 steel.
Shear Modulus 78.0 GPa11300 ksiEstimated from elastic modulus
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000248 ohm-cm
@Temperature 20.0 °C
0.0000248 ohm-cm
@Temperature 68.0 °F
 0.0000298 ohm-cm
@Temperature 100 °C
0.0000298 ohm-cm
@Temperature 212 °F
 0.0000552 ohm-cm
@Temperature 400 °C
0.0000552 ohm-cm
@Temperature 752 °F
 0.0000797 ohm-cm
@Temperature 600 °C
0.0000797 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.3 µm/m-°C
@Temperature -70.0 - 20.0 °C
6.28 µin/in-°F
@Temperature -94.0 - 68.0 °F
Austenitized 870°C (1600°F), 545°C (1010°F) temper for 2 hrs.
 12.4 µm/m-°C
@Temperature 21.0 - 260 °C
6.89 µin/in-°F
@Temperature 69.8 - 500 °F
Austenitized 870°C (1600°F), 545°C (1010°F) temper for 2 hrs.
 13.7 µm/m-°C
@Temperature 500 °C
7.61 µin/in-°F
@Temperature 932 °F
austenitized at 870°C (1600°F), 545°C (1010°F) temper for 2 hours
Specific Heat Capacity 0.475 J/g-°C0.114 BTU/lb-°FTypical 4000 series steel
Thermal Conductivity 44.5 W/m-K309 BTU-in/hr-ft²-°FTypical steel
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.37 - 0.44 %0.37 - 0.44 %
Chromium, Cr 0.65 - 0.95 %0.65 - 0.95 %
Iron, Fe 95.015 - 96.48 %95.015 - 96.48 %As remainder
Manganese, Mn 0.60 - 0.95 %0.60 - 0.95 %
Molybdenum, Mo 0.20 - 0.30 %0.20 - 0.30 %
Nickel, Ni 1.55 - 2.0 %1.55 - 2.0 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si 0.15 - 0.30 %0.15 - 0.30 %
Sulfur, S <= 0.020 %<= 0.020 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 4340 Steel, oil quenched 800°C (1470°F), 595°C (1100°F) temper, 25 mm round
AISI E4340 Steel, oil quenched 800°C (1470°F), 595°C (1100°F) temper, 25 mm round
AISI E4340 Steel, quenched 845°C, 315°C (600°F) temper
AISI E4340 Steel, quenched 845°C, 425°C (800°F) temper
AISI 4340 Steel, oil quenched 800°C (1470°F), 540°C (1000°F) temper, 25 mm round

M434EJ / 7827

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.