Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 2.25 g/cc | 2.25 g/cc |
Filler Content | 22.2 % | 22.2 % |
| 25 % | 25 % |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore D | 55 | 55 |
Tensile Strength | 6.89 - 11.0 MPa | 1000 - 1600 psi |
| 12.4 - 19.3 MPa | 1800 - 2800 psi |
Tensile Stress at Strain | 0.588 MPa @Strain 1 %, Temperature 250 °C | 85.3 psi @Strain 1 %, Temperature 482 °F |
| 0.785 MPa @Strain 1 %, Temperature 220 °C | 114 psi @Strain 1 %, Temperature 428 °F |
| 0.981 MPa @Strain 1 %, Temperature 180 °C | 142 psi @Strain 1 %, Temperature 356 °F |
| 1.08 MPa @Strain 2 %, Temperature 250 °C | 156 psi @Strain 2 %, Temperature 482 °F |
| 1.47 MPa @Strain 2 %, Temperature 220 °C | 213 psi @Strain 2 %, Temperature 428 °F |
| 1.67 MPa @Strain 3 %, Temperature 250 °C | 242 psi @Strain 3 %, Temperature 482 °F |
| 1.67 MPa @Strain 1 %, Temperature 140 °C | 242 psi @Strain 1 %, Temperature 284 °F |
| 1.96 MPa @Strain 2 %, Temperature 180 °C | 284 psi @Strain 2 %, Temperature 356 °F |
| 2.16 MPa @Strain 4 %, Temperature 250 °C | 313 psi @Strain 4 %, Temperature 482 °F |
| 2.16 MPa @Strain 3 %, Temperature 220 °C | 313 psi @Strain 3 %, Temperature 428 °F |
| 2.65 MPa @Strain 1 %, Temperature 100 °C | 384 psi @Strain 1 %, Temperature 212 °F |
| 2.75 MPa @Strain 4 %, Temperature 220 °C | 398 psi @Strain 4 %, Temperature 428 °F |
| 2.75 MPa @Strain 3 %, Temperature 180 °C | 398 psi @Strain 3 %, Temperature 356 °F |
| 3.14 MPa @Strain 2 %, Temperature 140 °C | 455 psi @Strain 2 %, Temperature 284 °F |
| 3.53 MPa @Strain 4 %, Temperature 180 °C | 512 psi @Strain 4 %, Temperature 356 °F |
| 3.63 MPa @Strain 1 %, Temperature 60.0 °C | 526 psi @Strain 1 %, Temperature 140 °F |
| 4.22 MPa @Strain 3 %, Temperature 140 °C | 612 psi @Strain 3 %, Temperature 284 °F |
| 4.61 MPa @Strain 2 %, Temperature 100 °C | 668 psi @Strain 2 %, Temperature 212 °F |
| 5.20 MPa @Strain 4 %, Temperature 140 °C | 754 psi @Strain 4 %, Temperature 284 °F |
| 5.88 MPa @Strain 2 %, Temperature 60.0 °C | 853 psi @Strain 2 %, Temperature 140 °F |
| 5.98 MPa @Strain 3 %, Temperature 100 °C | 868 psi @Strain 3 %, Temperature 212 °F |
| 6.18 MPa @Strain 1 %, Temperature 20.0 °C | 896 psi @Strain 1 %, Temperature 68.0 °F |
| 6.96 MPa @Strain 4 %, Temperature 100 °C | 1010 psi @Strain 4 %, Temperature 212 °F |
| 7.35 MPa @Strain 3 %, Temperature 60.0 °C | 1070 psi @Strain 3 %, Temperature 140 °F |
| 8.43 MPa @Strain 4 %, Temperature 60.0 °C | 1220 psi @Strain 4 %, Temperature 140 °F |
| >= 8.73 MPa @Strain 4 %, Temperature 20.0 °C | >= 1270 psi @Strain 4 %, Temperature 68.0 °F |
| >= 8.73 MPa @Strain 3 %, Temperature 20.0 °C | >= 1270 psi @Strain 3 %, Temperature 68.0 °F |
| 8.73 MPa @Strain 2 %, Temperature 20.0 °C | 1270 psi @Strain 2 %, Temperature 68.0 °F |
Elongation at Break | 100 - 200 % | 100 - 200 % |
| 200 - 300 % | 200 - 300 % |
Coefficient of Friction, Dynamic | 0.11 | 0.11 |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | >= 2.00e+15 ohm-cm | >= 2.00e+15 ohm-cm |
Surface Resistance | 1.00e+15 ohm | 1.00e+15 ohm |
| 1.00e+15 ohm | 1.00e+15 ohm |
Dielectric Constant | 2.2 - 2.5 @Frequency 100000 - 1.00e+7 Hz | 2.2 - 2.5 @Frequency 100000 - 1.00e+7 Hz |
| 2.2 - 2.5 @Frequency 100000 - 1.00e+7 Hz | 2.2 - 2.5 @Frequency 100000 - 1.00e+7 Hz |
Dielectric Loss Index | 0.00097 @Frequency 10000 Hz | 0.00097 @Frequency 10000 Hz |
| 0.0017 @Frequency 1000 Hz | 0.0017 @Frequency 1000 Hz |
| 0.062 @Frequency 1e+6 Hz | 0.062 @Frequency 1e+6 Hz |
| 0.225 @Frequency 100000 Hz | 0.225 @Frequency 100000 Hz |
| 0.28 @Frequency 10000 Hz | 0.28 @Frequency 10000 Hz |
| 0.39 @Frequency 1000 Hz | 0.39 @Frequency 1000 Hz |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 67.14 µm/m-°C @Temperature 30.0 - 250 °C | 37.30 µin/in-°F @Temperature 86.0 - 482 °F |
| 67.69 µm/m-°C @Temperature 30.0 - 200 °C | 37.61 µin/in-°F @Temperature 86.0 - 392 °F |
| 68.17 µm/m-°C @Temperature 30.0 - 150 °C | 37.87 µin/in-°F @Temperature 86.0 - 302 °F |
| 68.59 µm/m-°C @Temperature 30.0 - 100 °C | 38.11 µin/in-°F @Temperature 86.0 - 212 °F |
| 68.72 µm/m-°C @Temperature 15.0 - 30.0 °C | 38.18 µin/in-°F @Temperature 59.0 - 86.0 °F |
| 68.86 µm/m-°C @Temperature 30.0 - 50.0 °C | 38.26 µin/in-°F @Temperature 86.0 - 122 °F |
| 69.0 µm/m-°C @Temperature -60.0 - 15.0 °C | 38.3 µin/in-°F @Temperature -76.0 - 59.0 °F |
CTE, linear, Transverse to Flow | 62.46 µm/m-°C @Temperature 30.0 - 250 °C | 34.70 µin/in-°F @Temperature 86.0 - 482 °F |
| 63.04 µm/m-°C @Temperature 30.0 - 200 °C | 35.02 µin/in-°F @Temperature 86.0 - 392 °F |
| 63.36 µm/m-°C @Temperature 30.0 - 150 °C | 35.20 µin/in-°F @Temperature 86.0 - 302 °F |
| 63.68 µm/m-°C @Temperature 30.0 - 100 °C | 35.38 µin/in-°F @Temperature 86.0 - 212 °F |
| 63.87 µm/m-°C @Temperature 15.0 - 30.0 °C | 35.48 µin/in-°F @Temperature 59.0 - 86.0 °F |
| 63.87 µm/m-°C @Temperature 30.0 - 50.0 °C | 35.48 µin/in-°F @Temperature 86.0 - 122 °F |
| 64.0 µm/m-°C @Temperature -60.0 - 15.0 °C | 35.6 µin/in-°F @Temperature -76.0 - 59.0 °F |
Thermal Conductivity | 0.375 W/m-K | 2.60 BTU-in/hr-ft²-°F |
Maximum Service Temperature, Air | 260 °C | 500 °F |
Minimum Service Temperature, Air | -250 °C | -418 °F |