Physical Properties | Metric | English | Comments |
---|
Density | 2.66 g/cc | 0.0961 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 58 | 58 |
Hardness, Knoop | 73 | 73 |
Tensile Strength, Ultimate | 241 MPa | 35000 psi |
| 41.0 MPa @Temperature 371 °C | 5950 psi @Temperature 700 °F |
| 75.0 MPa @Temperature 316 °C | 10900 psi @Temperature 601 °F |
| 115 MPa @Temperature 260 °C | 16700 psi @Temperature 500 °F |
| 150 MPa @Temperature 204 °C | 21800 psi @Temperature 399 °F |
| 200 MPa @Temperature 149 °C | 29000 psi @Temperature 300 °F |
| 240 MPa @Temperature -28.0 °C | 34800 psi @Temperature -18.4 °F |
| 240 MPa @Temperature 24.0 °C | 34800 psi @Temperature 75.2 °F |
| 240 MPa @Temperature 100 °C | 34800 psi @Temperature 212 °F |
| 250 MPa @Temperature -80.0 °C | 36300 psi @Temperature -112 °F |
| 360 MPa @Temperature -196 °C | 52200 psi @Temperature -321 °F |
Tensile Strength, Yield | 117 MPa | 17000 psi |
| 29.0 MPa @Temperature 371 °C | 4210 psi @Temperature 700 °F |
| 50.0 MPa @Temperature 316 °C | 7250 psi @Temperature 601 °F |
| 75.0 MPa @Temperature 260 °C | 10900 psi @Temperature 500 °F |
| 105 MPa @Temperature 204 °C | 15200 psi @Temperature 399 °F |
| 110 MPa @Temperature 149 °C | 16000 psi @Temperature 300 °F |
| 115 MPa @Temperature -80.0 °C | 16700 psi @Temperature -112 °F |
| 115 MPa @Temperature -28.0 °C | 16700 psi @Temperature -18.4 °F |
| 115 MPa @Temperature 24.0 °C | 16700 psi @Temperature 75.2 °F |
| 115 MPa @Temperature 100 °C | 16700 psi @Temperature 212 °F |
| 130 MPa @Temperature -196 °C | 18900 psi @Temperature -321 °F |
Elongation at Break | 30 % @Temperature 24.0 °C | 30 % @Temperature 75.2 °F |
| 32 % @Temperature -28.0 °C | 32 % @Temperature -18.4 °F |
| 35 % @Temperature -80.0 °C | 35 % @Temperature -112 °F |
| 36 % @Temperature 100 °C | 36 % @Temperature 212 °F |
| 46 % @Temperature -196 °C | 46 % @Temperature -321 °F |
| 50 % @Temperature 149 °C | 50 % @Temperature 300 °F |
| 60 % @Temperature 204 °C | 60 % @Temperature 399 °F |
| 80 % @Temperature 260 °C | 80 % @Temperature 500 °F |
| 110 % @Temperature 316 °C | 110 % @Temperature 601 °F |
| 130 % @Temperature 371 °C | 130 % @Temperature 700 °F |
| 27 % @Thickness 1.59 mm | 27 % @Thickness 0.0625 in |
Modulus of Elasticity | 70.3 GPa | 10200 ksi |
Poissons Ratio | 0.33 | 0.33 |
Fatigue Strength | 117 MPa @# of Cycles 5.00e+8 | 17000 psi @# of Cycles 5.00e+8 |
Machinability | 30 % | 30 % |
Shear Modulus | 26.0 GPa | 3770 ksi |
Shear Strength | 152 MPa | 22000 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000532 ohm-cm @Temperature 20.0 °C | 0.00000532 ohm-cm @Temperature 68.0 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 22.1 µm/m-°C @Temperature -50.0 - 20.0 °C | 12.3 µin/in-°F @Temperature -58.0 - 68.0 °F |
| 23.9 µm/m-°C @Temperature 20.0 - 100 °C | 13.3 µin/in-°F @Temperature 68.0 - 212 °F |
| 24.0 µm/m-°C @Temperature 20.0 - 100 °C | 13.3 µin/in-°F @Temperature 68.0 - 212 °F |
| 24.9 µm/m-°C @Temperature 20.0 - 200 °C | 13.8 µin/in-°F @Temperature 68.0 - 392 °F |
| 25.9 µm/m-°C @Temperature 20.0 - 300 °C | 14.4 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.900 J/g-°C | 0.215 BTU/lb-°F |
Thermal Conductivity | 125 W/m-K | 870 BTU-in/hr-ft²-°F |
Melting Point | 593 - 643 °C | 1100 - 1190 °F |
Solidus | 593 °C | 1100 °F |
Liquidus | 643 °C | 1190 °F |
|
Processing Properties | Metric | English | Comments |
---|
Annealing Temperature | 343 °C | 650 °F |
Hot-Working Temperature | 260 - 510 °C | 500 - 950 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 94.8 - 96.8 % | 94.8 - 96.8 % |
Chromium, Cr | 0.15 - 0.35 % | 0.15 - 0.35 % |
Copper, Cu | <= 0.05 % | <= 0.05 % |
Magnesium, Mg | 3.1 - 3.9 % | 3.1 - 3.9 % |
Manganese, Mn | <= 0.01 % | <= 0.01 % |
Other, each | <= 0.05 % | <= 0.05 % |
Other, total | <= 0.15 % | <= 0.15 % |
Si+Fe | <= 0.45 % | <= 0.45 % |
Titanium, Ti | <= 0.05 % | <= 0.05 % |
Zinc, Zn | <= 0.20 % | <= 0.20 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.