MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Thermx® FG30GT NC010 PCT  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polycyclohexylenedimethylene Terephthalate (PCT); Polycyclohexylenedimethylene Terephthalate (PCT), 30% Glass Reinforced

Material Notes: Thermx® FG30GT NC010 is a 30% glass fiber reinforced, toughened modified polycyclohexylenedimethylene terephthalate resin suitable for repeated-use food-contact US FDA housewares applications.

Celenese acquired the Thermx product line from DuPont in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.41 g/cc1.41 g/ccASTM D 792
Density 1.40 g/cc0.0506 lb/in³ISO 1183
Filler Content 30 %30 %Glass fiber reinforcement
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 113113ASTM D 785
Tensile Strength at Break  97.0 MPa
@Temperature 23.0 °C
14100 psi
@Temperature 73.4 °F
ASTM D 638
 105 MPa
@Temperature 23.0 °C
15200 psi
@Temperature 73.4 °F
ISO 527
Elongation at Break  2.5 %
@Temperature 23.0 °C
2.5 %
@Temperature 73.4 °F
ISO 527
 3.1 %
@Temperature 23.0 °C
3.1 %
@Temperature 73.4 °F
ASTM D 638
Tensile Modulus 7.80 GPa
@Temperature 23.0 °C
1130 ksi
@Temperature 73.4 °F
ISO 527
Flexural Strength  157 MPa
@Temperature 23.0 °C
22800 psi
@Temperature 73.4 °F
ASTM D 790
 160 MPa
@Temperature 23.0 °C
23200 psi
@Temperature 73.4 °F
ISO 178
Flexural Modulus  6.77 GPa
@Temperature 23.0 °C
982 ksi
@Temperature 73.4 °F
ASTM D 790
 6.80 GPa
@Temperature 23.0 °C
986 ksi
@Temperature 73.4 °F
ISO 178
Izod Impact, Notched  1.10 J/cm
@Temperature -40.0 °C
2.06 ft-lb/in
@Temperature -40.0 °F
ASTM D 256
 1.50 J/cm
@Temperature 23.0 °C
2.81 ft-lb/in
@Temperature 73.4 °F
ASTM D 256
Izod Impact, Unnotched 9.10 J/cm
@Temperature 23.0 °C
17.0 ft-lb/in
@Temperature 73.4 °F
ASTM D 4812
Izod Impact, Notched (ISO) 10.0 kJ/m²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched 5.00 J/cm²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched 1.00 J/cm²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 283 °C541 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 268 °C514 °FASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 221 °C430 °FASTM D 648
 232 °C450 °FISO 75-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 300 °C572 °FOptimum
 295 - 310 °C563 - 590 °F
Mold Temperature 160 °C320 °FOptimum
 150 - 175 °C302 - 347 °F
Drying Temperature 120 - 150 °C248 - 302 °F
Dry Time 4 - 6 hour4 - 6 hourDehumidified Dryer
Moisture Content <= 0.030 %<= 0.030 %
 
Descriptive Properties
AppearanceNatural Color
DuPont Product CategoryFood Contact Resins
 Glass Reinforced Resins
 Toughened Resins
FeaturesFood Contact Acceptable
 Toughness, Good
FormPellets
Part Marking Code>PCT-IGF30<ISO 11469
Processing MethodInjection Molding
RegionAmericas
 Asia/Pacific
 Europe
Resin IdentificationPCT-IGF30ISO 1043
UsesFood Applications, Non-specific
 Food Service Applications

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Thermx® FG15 NC010 15% Glass Reinforced, Food Grade PCT Resin
BASF Ultradur® B 4040 G6 30% Glass Filled PBT + PET
Overview of materials for Polycyclohexylenedimethylene Terephthalate (PCT), 30% Glass Reinforced
Lotte Advanced Materials Infino® TK-2046H PCT, Glass Filled
E-Polymers TEKALOY® F50G30 30% Glass Fiber Reinforced PBT/PET Alloy

PDTA8723 / 31756

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.