MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Trinseo CALIBRE™ 201-22 Polycarbonate Resin
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: CALIBRE™ 200-22 polycarbonate resins are produced in compliance with the US FDA and EU food contact regulations. They provide excellent impact resistance, heat distortion resistance and optical clarity. The CALIBRE™ 200-22 series products are available in 4 additive packages: CALIBRE 200: No mold release or UV Stabilizer. CALIBRE 201: Mold release. CALIBRE 202: UV Stabilizer. CALIBRE 203: Mold release and UV stabilizer. (Not that CALIBRE 202 and 203 grades are not available in Europe and do not comply with EU food contact regulations).

Applications:

  • Food processors
  • Beverage containers
  • Food utensils
  • Other packaging applications
Govt. and Industry Standards:
  • US FDA 21 CFR 177.1580
  • CSA
  • Underwriters Laboratory (UL)
  • EU food contact 2002/72/EC

Information provided by Trinseo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ISO 1183/A
Water Absorption 0.15 %
@Time 86400 sec
0.15 %
@Time 24.0 hour
ISO 62
Moisture Absorption at Equilibrium 0.32 %0.32 %50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inISO 294-4
Melt Flow 22 g/10 min
@Load 1.20 kg,
Temperature 300 °C
22 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7272ASTM D785
Hardness, Rockwell R 118118ASTM D785
Tensile Strength at Break 65.5 MPa9500 psi50 mm/min; ASTM D638
 66.0 MPa9570 psiISO 527-2/50
Tensile Strength, Yield 60.0 MPa8700 psi50 mm/min; ASTM D638
 60.0 MPa8700 psiISO 527-2/50
Elongation at Break 120 %120 %50 mm/min; ASTM D638
 120 %120 %ISO 527-2/50
Tensile Modulus 2.30 GPa334 ksiISO 527-2/50
 2.34 GPa339 ksi50 mm/min; ASTM D638
Flexural Strength 96.5 MPa14000 psiMethod I (3 point load), 2.0 mm/min; ASTM D790
 97.0 MPa14100 psi2.0 mm/min; ISO 178
Flexural Modulus 2.40 GPa348 ksi2.0 mm/min; ISO 178
 2.41 GPa350 ksiMethod I (3 point load), 2.0 mm/min; ASTM D790
Izod Impact, Notched 7.50 J/cm14.1 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 74.0 kJ/m²35.2 ft-lb/in²ISO 180/A
Izod Impact, Unnotched (ISO) NBNBISO 180
Tensile Impact Strength 378 kJ/m²180 ft-lb/in²ASTM D1822
Dart Drop, Total Energy 72.3 J53.3 ft-lb3.39 m/sec; ASTM D3763
Abrasion 4545[%], Taber; ASTM D1044
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2.00e+17 ohm-cm2.00e+17 ohm-cmASTM D257
Dielectric Constant  3.0
@Frequency 60 Hz
3.0
@Frequency 60 Hz
ASTM D150
 3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 17.0 kV/mm432 kV/inASTM D149
Dissipation Factor  0.0010
@Frequency 50 Hz
0.0010
@Frequency 50 Hz
ASTM D150
 0.0020
@Frequency 1e+6 Hz
0.0020
@Frequency 1e+6 Hz
ASTM D150
Comparative Tracking Index 250 V
@Thickness 2.00 mm
250 V
@Thickness 0.0787 in
Solution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 68.0 µm/m-°C
@Temperature -40.0 - 82.0 °C
37.8 µin/in-°F
@Temperature -40.0 - 180 °F
ASTM D696
Hot Ball Pressure Test 125 °C257 °FIEC 60335-1
Deflection Temperature at 0.46 MPa (66 psi) 139 °C282 °FUnannealed; ISO 75-2/B
 142 °C288 °FAnnealed; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 126 °C259 °FUnannealed; ASTM D648
 126 °C259 °FAnnealed; ISO 75-2/A
 139 °C282 °FAnnealed; ASTM D648
Vicat Softening Point 147 °C297 °FISO 306/B50
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
Oxygen Index 26 %26 %ISO 4589-2
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5861.586ISO 489
Haze <= 1.0 %<= 1.0 %ASTM D1003
Transmission, Visible 89 %89 %ASTM D1003
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Delrin Delrin® 500P NC010 POM
Trinseo CALIBRE™ 200 22 Polycarbonate, General Purpose
Covestro Makrolon® 2458 Polycarbonate, Injection Grade
Trinseo CALIBRE™ 2061-15 Polycarbonate Resin
Trinseo CALIBRE™ 201-6 Polycarbonate Resin

PDWST012 / 142221

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.