MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Titanium Grade 12
Categories: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium

Material Notes: Addition of 0.3% Mo and 0.8% Ni to titanium increases corrosion resistance at a lower cost than Pd (see Ti Grades 7 and 11). Higher strength than unalloyed Ti grades 1 - 4, yet still formable.

Microstructure: Equiaxed alpha, with acicular alpha, primarily in welds or heat-affected zones, small amounts of beta.

Applications: Chemical processing, in mildly reducing or variable oxidizing-reducing media - containers, heat exchangers, pumps, valves, pipes and fittings.

Forms typically available: billet, bar, rod, plate, sheet, strip and tubing.

Titanium Grades 1,2,3,4,7,11,and 12 are all considered unalloyed and have similar mechanical properties.

Key Words: UNS R53400; ASTM Grade 12, titanium alloy
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.50 g/cc0.163 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 180 - 235180 - 235
Hardness, Knoop 222222Estimated from Brinell.
Hardness, Rockwell C 1111Converted from Brinell hardness. Value below normal HRC range, for comparison purposes only.
Hardness, Vickers 209209Estimated from Brinell.
Tensile Strength 550 MPa79800 psiWeld strength in 13 mm plate
 325 MPa
@Temperature 316 °C
47100 psi
@Temperature 601 °F
 345 MPa
@Temperature 240 °C
50000 psi
@Temperature 464 °F
 510 MPa
@Temperature 25.0 °C
74000 psi
@Temperature 77.0 °F
Tensile Strength, Ultimate 450 MPa65300 psi
Tensile Strength, Yield 380 MPa55100 psi
 205 MPa
@Temperature 316 °C
29700 psi
@Temperature 601 °F
0.2% offset
 250 MPa
@Temperature 240 °C
36300 psi
@Temperature 464 °F
0.2% offset
 415 MPa
@Temperature 25.0 °C
60200 psi
@Temperature 77.0 °F
0.2% offset
Elongation at Break 12 %12 %Weld elongation in 13 mm plate
 32 %
@Temperature 316 °C
32 %
@Temperature 601 °F
 33 %
@Temperature 25.0 °C
33 %
@Temperature 77.0 °F
 37 %
@Temperature 240 °C
37 %
@Temperature 464 °F
Creep Strength  48.0 MPa
@Temperature 315 °C,
Time 1.80e+7 - 3.60e+7 sec
6960 psi
@Temperature 599 °F,
Time 5000 - 10000 hour
Creep strain rate 0.0000033 %/hour
 138 MPa
@Temperature 315 °C,
Time 1.80e+7 - 3.60e+7 sec
20000 psi
@Temperature 599 °F,
Time 5000 - 10000 hour
Creep strain rate 0.0000186 %/hour
 138 MPa
@Temperature 25.0 °C,
Time 1.80e+7 - 3.60e+7 sec
20000 psi
@Temperature 77.0 °F,
Time 5000 - 10000 hour
Creep strain rate 0 %/hour
 331 MPa
@Temperature 25.0 °C,
Time 1.80e+7 - 3.60e+7 sec
48000 psi
@Temperature 77.0 °F,
Time 5000 - 10000 hour
Creep strain rate 0.0000394 %/hour
Tensile Modulus 105 GPa15200 ksi
Compressive Modulus 110 GPa16000 ksi
Poissons Ratio 0.370.37
Fatigue Strength  160 MPa
@# of Cycles 100000
23200 psi
@# of Cycles 100000
Reverse bending, 1.3mm sheet, notched (Kt = 3.5)
 345 MPa
@# of Cycles 1.00e+6
50000 psi
@# of Cycles 1.00e+6
Reverse bending, 1.3mm sheet
Shear Modulus 45.0 GPa6530 ksi
Charpy Impact 15.0 J11.1 ft-lb
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000520 ohm-cm0.0000520 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 325 J/g140 BTU/lbHigh Purity Ti.
CTE, linear  8.60 µm/m-°C
@Temperature 0.000 - 100 °C
4.78 µin/in-°F
@Temperature 32.0 - 212 °F
 9.50 µm/m-°C
@Temperature 0.000 - 315 °C
5.28 µin/in-°F
@Temperature 32.0 - 599 °F
average
Specific Heat Capacity  0.555 J/g-°C
@Temperature 23.0 °C
0.133 BTU/lb-°F
@Temperature 73.4 °F
 0.670 J/g-°C
@Temperature 540 °C
0.160 BTU/lb-°F
@Temperature 1000 °F
Thermal Conductivity 19.0 W/m-K132 BTU-in/hr-ft²-°Fannealed
Melting Point <= 1660 °C<= 3020 °F
Liquidus 1660 °C3020 °F
Maximum Service Temperature, Air 425 °C797 °FContinuous use
 540 °C1000 °FIntermittent Use
Beta Transus 890 °C1630 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.30
@Temperature 710 °C
0.30
@Temperature 1310 °F
High purity Ti
Reflection Coefficient, Visible (0-1) 0.560.56High purity Ti; visible light.
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe <= 0.30 %<= 0.30 %
Molybdenum, Mo 0.20 - 0.40 %0.20 - 0.40 %
Nickel, Ni 0.60 - 0.90 %0.60 - 0.90 %
Nitrogen, N <= 0.030 %<= 0.030 %
Other, each <= 0.050 %<= 0.050 %
 <= 0.050 %<= 0.050 %
Other, total <= 0.30 %<= 0.30 %
 <= 0.30 %<= 0.30 %
Oxygen, O <= 0.25 %<= 0.25 %
Titanium, Ti 97.725 - 99.2 %97.725 - 99.2 %As Balance; Elemental Composition per ASTM B265

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Grade 7
Titanium Grade 2
Titanium Grade 11
Titanium Grade 4
Titanium Grade 1

MTU120 / 14268

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.