MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont Mobility and Materials Hytrel® HTR8139BK TPC-ET  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: 44 Shore D, Lubricated, High Viscosity Polyester Elastomer Developed for Blow Molding

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.15 g/cc0.0415 lb/in³ISO 1183
Melt Density 0.960 g/cc
@Temperature >=194 °C
0.0347 lb/in³
@Temperature >=381 °F
Water Absorption 0.70 %
@Time 86400 sec
0.70 %
@Time 24.0 hour
Sim. to ISO 62
 0.70 %
@Thickness 2.00 mm
0.70 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
0.200 %
@Thickness 0.0787 in
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.016 cm/cm0.016 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.014 cm/cm0.014 in/inISO 294-4, 2577
Melt Flow  2.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
2.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
from MVR and melt density; ISO 1133
 2.1 g/10 min
@Load 2.16 kg,
Temperature 230 °C
2.1 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4444ISO 7619-1
 40
@Time 15.0 sec
40
@Time 0.00417 hour
ISO 7619-1
Tensile Strength at Break 32.0 MPa4640 psiISO 527-1/-2
Tensile Stress at Strain  4.50 MPa
@Strain 5.0 %
653 psi
@Strain 5.0 %
ISO 527-1/-2
 6.70 MPa
@Strain 10 %
972 psi
@Strain 10 %
ISO 527-1/-2
 11.8 MPa
@Strain 50 %
1710 psi
@Strain 50 %
ISO 527-1/-2
 14.0 MPa
@Strain 100 %
2030 psi
@Strain 100 %
ISO 527-1/-2
 23.0 MPa
@Strain 300 %
3340 psi
@Strain 300 %
ISO 527-1/-2
Elongation at Break >= 300 %>= 300 %ISO 527-1/-2
 510 %510 %ISO 527-1/-2
Tensile Modulus 0.0550 GPa7.98 ksiISO 527-1/-2
Flexural Modulus 0.0870 GPa12.6 ksiISO 178
Izod Impact, Unnotched (ISO)  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 180/1A
 NB
@Temperature -40.0 °C
NB
@Temperature -40.0 °F
ISO 180/1A
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eA
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eA
 NB
@Temperature -40.0 °C
NB
@Temperature -40.0 °F
ISO 179/1eA
Tear Strength 110 kN/m628 pliparallel; ISO 34-1
 120 kN/m685 plinormal; ISO 34-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 4.00e+13 ohm-cm4.00e+13 ohm-cmIEC 62631-3-1
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 62631-3-2
Dielectric Constant  4.6
@Frequency 1e+6 Hz
4.6
@Frequency 1e+6 Hz
IEC 62631-2-1
 4.9
@Frequency 100 Hz
4.9
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 19.0 kV/mm483 kV/inIEC 60243-1
Dissipation Factor  0.0050
@Frequency 100 Hz
0.0050
@Frequency 100 Hz
IEC 62631-2-1
 0.0275
@Frequency 1e+6 Hz
0.0275
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 180 µm/m-°C100 µin/in-°FISO 11359-1/-2
 210 µm/m-°C
@Temperature -40.0 - 23.0 °C
117 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 170 µm/m-°C94.4 µin/in-°FISO 11359-1/-2
 200 µm/m-°C
@Temperature -40.0 - 23.0 °C
111 µin/in-°F
@Temperature -40.0 - 73.4 °F
ISO 11359-1/-2
Melting Point 194 °C381 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 58.0 °C136 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 44.0 °C111 °FISO 75-1/-2
Brittleness Temperature -100 °C-148 °FISO 974
Glass Transition Temp, Tg -45.0 °C-49.0 °F10°C/min; ISO 11357-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
Oxygen Index 21 %21 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 225 °C437 °FInjection Optimum
 220 - 240 °C428 - 464 °FInjection
Mold Temperature 40.0 - 50.0 °C104 - 122 °FInjection
 45.0 °C113 °FInjection Optimum
Drying Temperature 100 °C212 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.080 %0.080 %Injection
 
Descriptive Properties
AdditivesLubricants
Delivery formPellets
Drying RecommendedyesInjection
Eff. thermal diffusivity5.44E-08 m²/s
FMVSS ClassBISO 3795 (FMVSS 302)
Part Marking CodeTPC-ETISO 11469
ProcessingBlow Molding
 Injection Molding
 Thermoforming
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationTPC-ETISO 1043
Special characteristicsHeat stabilized or stable to heat
 Light stabilized or stable to light

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Hytrel® HTR8223 BK320 TPC-ET
Celanese Hytrel® 4556 TPC-ET
Celanese Hytrel® 6356 TPC-ET
Celanese Hytrel® HTR8068 TPC-ET-FR(17)
Celanese Hytrel® 4053FG NC010 TPC-ET

PDSX5208 / 197848

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.