MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

MRC Polymers NAXALOY™ 795 Polycarbonate & Polyester Blend  (discontinued **)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate/PET Polyester Blend; Polyester, TP

Material Notes: Polycarbonate & Polyester Blend

Mechanical properties measured on 1/8 in. (3.2 mm) samples.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.24 g/cc0.0448 lb/in³ASTM D792
Water Absorption 0.15 %0.15 %24 hours, ASTM D570
Linear Mold Shrinkage, Flow 0.0060 - 0.0080 cm/cm
@Thickness 3.17 mm
0.0060 - 0.0080 in/in
@Thickness 0.125 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0070 - 0.0090 cm/cm0.0070 - 0.0090 in/inASTM D955
Melt Flow 15 g/10 min
@Load 1.20 kg,
Temperature 300 °C
15 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 51.0 MPa7400 psiASTM D638
Elongation at Break 80 %80 %ASTM D638
Flexural Yield Strength 77.0 MPa11200 psiASTM D790
Flexural Modulus 1.929 GPa279.8 ksiASTM D790
Izod Impact, Notched 8.01 J/cm15.0 ft-lb/inASTM D256
Impact Test  20.3 J
@Temperature -30.0 °C
15.0 ft-lb
@Temperature -22.0 °F
ASTM D3763
 46.1 J
@Temperature 23.0 °C
34.0 ft-lb
@Temperature 73.4 °F
ASTM D3763
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 112 °C234 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °C194 °FUnannealed; ASTM D648
Flammability, UL94 HB
@Thickness 1.47 mm
HB
@Thickness 0.0579 in
UL Rating, File #E92442
 
Processing PropertiesMetricEnglishComments
Processing Temperature 249 - 260 °C480 - 500 °F
Rear Barrel Temperature 238 - 249 °C460 - 480 °F
Middle Barrel Temperature 243 - 255 °C469 - 491 °F
Front Barrel Temperature 249 - 265 °C480 - 509 °F
Nozzle Temperature 249 - 265 °C480 - 509 °F
Mold Temperature 38.0 - 71.0 °C100 - 160 °F
Drying Temperature 99.0 - 110 °C210 - 230 °F
Dry Time 6 - 8 hour6 - 8 hour
Moisture Content <= 0.010 %<= 0.010 %
Dew Point <= -17.8 °C<= 0.000 °F
Drying Air Flow Rate 22.7 - 28.3 l/min0.800 - 1.00 ft³/min (CFM)per lb/hour resin processed
Injection Pressure 34.5 - 172 MPa5000 - 25000 psi
Back Pressure 0.345 - 1.03 MPa50.0 - 150 psi
Cushion 0.635 cm0.250 in
Screw Speed 20 - 50 rpm20 - 50 rpm
 
Descriptive Properties
Fill RateModerate
Hold Pressure40 - 60% of injection pressure
Packing Pressure50 - 75% of injection pressure

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
MRC Polymers NAXALOY™ 780 GF11 PC+PBT Polyester Blend, 11% Glass Fiber Filled
MRC Polymers NAXALOY™ 794A1 Polycarbonate & Polyester Blend

PMRC956 / 21014

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.