MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teijin Panlite® L-1250J Polycarbonate, Hot Water Resistant Grade  (discontinued **)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, High Heat

Material Notes: Injection Molding.

Applications: Electric and and electronic appliance parts, machine parts, protective equipment parts, medical equipment, lighting fixtures requiring heat resistance and trasparency; tableware and mechanical parts requiring cold and heat resistance.

Key Words: PC
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ASTM D792
Water Absorption 0.20 %0.20 %23°C; 24 hr; ASTM D570
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7777ASTM D785
Tensile Strength, Ultimate 81.0 MPa11700 psiASTM D638
Tensile Strength, Yield 61.0 MPa8850 psiASTM D638
Elongation at Break 140 %140 %ASTM D638
Elongation at Yield 6.0 %6.0 %ASTM D638
Tensile Modulus 2.12 GPa307 ksiASTM D638
Flexural Yield Strength 90.0 MPa13100 psiASTM D790
Flexural Modulus 2.23 GPa323 ksiASTM D790
Compressive Yield Strength 76.0 MPa11000 psiASTM D695
Izod Impact, Notched  1.40 J/cm
@Thickness 6.40 mm
2.62 ft-lb/in
@Thickness 0.252 in
ASTM D256
 8.80 J/cm
@Thickness 3.20 mm
16.5 ft-lb/in
@Thickness 0.126 in
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 3.00e+16 ohm-cm3.00e+16 ohm-cmASTM D257
Dielectric Constant  2.9
@Frequency 60 Hz
2.9
@Frequency 60 Hz
ASTM D150
 2.95
@Frequency 1e+6 Hz
2.95
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 30.0 kV/mm
@Thickness 1.60 mm
762 kV/in
@Thickness 0.0630 in
quick pressure rise method; ASTM D149
Dissipation Factor  0.00040
@Frequency 60 Hz
0.00040
@Frequency 60 Hz
ASTM D150
 0.0090
@Frequency 1e+6 Hz
0.0090
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 110 sec110 secASTM D495
Comparative Tracking Index 300 V300 VIEC 112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
38.9 µin/in-°F
@Temperature 68.0 °F
ASTM D696
CTE, linear, Transverse to Flow 70.0 µm/m-°C
@Temperature 20.0 °C
38.9 µin/in-°F
@Temperature 68.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 143 °C289 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 133 °C271 °FASTM D648
UL RTI, Electrical 125 °C
@Thickness 1.47 mm
257 °F
@Thickness 0.0579 in
UL RTI, Mechanical with Impact 115 °C
@Thickness 1.47 mm
239 °F
@Thickness 0.0579 in
UL RTI, Mechanical without Impact 125 °C
@Thickness 1.47 mm
257 °F
@Thickness 0.0579 in
Flammability, UL94  V-2
@Thickness 1.47 mm
V-2
@Thickness 0.0579 in
 V-2
@Thickness 3.05 mm
V-2
@Thickness 0.120 in
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5851.585ASTM D542
Transmission, Visible 89 %
@Thickness 3.00 mm
89 %
@Thickness 0.118 in
ASTM D1003

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Moplen EP548P Polypropylene, Impact Modified; Molded/Extruded
PolyMirae Moplen EP548P Injection Molding Grade Polypropylene
LyondellBasell Moplen EP548Q Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Moplen EP548L Polypropylene, Impact Modified; Molded/Extruded
LyondellBasell Moplen EP548S Polypropylene, Impact Modified; Molded/Extruded

PLAT10 / 49990

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.