MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Alliance Polymers Viprene™ G75A-32U-NAT Thermoplastic Vulcanizate Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Viprene™ G75A-32U-NAT is a UV and Heat Stabilized TVP (Thermoplastic Vulcanizate Elastomer). This material can be easily processed by extrusion or injection molding. It exhibits easy flowing characteristics.

Availability: North America

Additive: Heat Stabilizer and UV Stabilizer

Features: Good Flow, Good UV Resistance and Heat Stabilized

Appearance: Natural Color

Forms: Pellets

Processing Method: Extrusion and Injection Molding

Information provided by Alliance Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.970 g/cc0.0350 lb/in³ISO 2781
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7575ISO 868
Tensile Strength at Break 8.48 MPa1230 psiISO 37
Tensile Stress at Strain  2.90 MPa
@Strain 100 %
421 psi
@Strain 100 %
ISO 37
 4.20 MPa
@Strain 300 %
609 psi
@Strain 300 %
ISO 37
Elongation at Break 550 %550 %ISO 37
Tear Strength 45.6 kN/m260 pliISO 34-1
Compression Set 43 %
@Temperature 70.0 °C,
Time 79200 sec
43 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D3995B
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -60.0 °C-76.0 °FASTM D746
Flammability, UL94  HB
@Thickness 1.00 mm
HB
@Thickness 0.0394 in
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 195 °C383 °FGate Temperature; Extrusion
 190 - 230 °C374 - 446 °FInjection
Rear Barrel Temperature 180 °C356 °FInjection
Middle Barrel Temperature 185 °C365 °FInjection
Front Barrel Temperature 185 °C365 °FInjection
Nozzle Temperature 190 - 220 °C374 - 428 °FInjection
Zone 1 180 °C356 °FExtrusion
Zone 2 185 °C365 °FExtrusion
Zone 3 185 °C365 °FExtrusion
Die Temperature 200 °C
@Pressure 4.80 - 17.0 MPa
392 °F
@Pressure 696 - 2470 psi
Extrusion
Mold Temperature 10.0 - 50.0 °C50.0 - 122 °FInjection
Injection Velocity >= 50.0 mm/sec>= 1.97 in/secInjection
Drying Temperature 80.0 °C176 °FInjection
 80.0 °C176 °FExtrusion
Dry Time 3.00 hour3.00 hourInjection
 3.00 hour3.00 hourExtrusion
Back Pressure 0.500 - 0.848 MPa72.5 - 123 psiInjection
Clamp Pressure 40.0 - 70.3 MPa5800 - 10200 psiInjection
Screw Speed 100 - 200 rpm100 - 200 rpmInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman Diamond Softflex® SF 0450
LyondellBasell Hifax TRC 779X BLACK Thermoplastic Olefinic Elastomer, mineral Filled
ExxonMobil Santoprene® 912BA Thermoplastic Elastomer
ExxonMobil Santoprene® 8221-70 Thermoplastic Elastomer
Dow INFUSE™ 9500 Olefin Block Copolymer

PAPS020 / 159393

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.