MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Desmopan® 9392A GMP TPU
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Extrusion- and injection molding grade; very good hydrolysis and microbial resistance; good low-temperature flexibility; complies with VDE 0282-10; Application; Cable sheathings; Hoses, non-reinforced

Mechanical property data for samples at 50% RH.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.15 g/cc1.15 g/ccISO 1183-1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9292ISO 868
Hardness, Shore D 4242ISO 868
Tensile Strength, Ultimate 50.0 MPa7250 psi200 mm/min; b.o. ISO 527-1,-3
Tensile Stress at Strain  11.0 MPa
@Strain 100 %
1600 psi
@Strain 100 %
200 mm/min; b.o. ISO 527-1,-3
 30.0 MPa
@Strain 300 %
4350 psi
@Strain 300 %
200 mm/min; b.o. ISO 527-1,-3
Elongation at Break 400 %400 %200 mm/min; b.o. ISO 527-1,-3
Tensile Modulus  0.0710 GPa
@Temperature 60.0 °C
10.3 ksi
@Temperature 140 °F
storage; ISO 6721-1,-4
 0.132 GPa
@Temperature 20.0 °C
19.1 ksi
@Temperature 68.0 °F
storage; ISO 6721-1,-4
 0.700 GPa
@Temperature -20.0 °C
102 ksi
@Temperature -4.00 °F
storage; ISO 6721-1,-4
Flexural Modulus  0.0130 GPa
@Temperature 70.0 °C
1.89 ksi
@Temperature 158 °F
Torsional storage; ISO 6721-2
 0.0220 GPa
@Temperature 23.0 °C
3.19 ksi
@Temperature 73.4 °F
Torsional storage; ISO 6721-2
 0.104 GPa
@Temperature -20.0 °C
15.1 ksi
@Temperature -4.00 °F
Torsional storage; ISO 6721-2
Rebound 32 %32 %Resilience; ISO 4662
Tear Strength 85.0 kN/m485 pli500 mm/min; ISO 34-1
Abrasion 2020mm3; ISO 4649 method A
Compression Set  20 %
@Temperature 23.0 °C,
Time 259000 sec
20 %
@Temperature 73.4 °F,
Time 72.0 hour
ISO 815
 37 %
@Temperature 70.0 °C,
Time 86400 sec
37 %
@Temperature 158 °F,
Time 24.0 hour
DIN ISO 815-1, Method C
 55 %
@Temperature 70.0 °C,
Time 86400 sec
55 %
@Temperature 158 °F,
Time 24.0 hour
ISO 815
 
Processing PropertiesMetricEnglishComments
Melt Temperature 195 - 215 °C383 - 419 °FExtrusion
 210 - 230 °C410 - 446 °FInjection
Mold Temperature 20.0 - 40.0 °C68.0 - 104 °F
Drying Temperature 80.0 °C176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Desmopan® 2792A GMP TPU
Covestro Desmopan® 9392AU Polyurethane
DSM Biomedical Bionate® II 55D Thermoplastic Polycarbonate Polyurethane (PCU)
Covestro Desmopan® 1092A TPU
AorTech Biomaterials Elast-Eon™ E2A Biomedical Polyurethane Pellets

PCOVEST0723 / 202506

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.