MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polyether Ester Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester, TP; Polyether Ester Elastomer

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyether Ester Elastomer". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.05 - 1.48 g/cc0.0379 - 0.0535 lb/in³Average value: 1.20 g/cc Grade Count:156
Water Absorption 0.100 - 7.00 %0.100 - 7.00 %Average value: 0.975 % Grade Count:73
Moisture Absorption at Equilibrium 0.150 - 0.580 %0.150 - 0.580 %Average value: 0.297 % Grade Count:27
Linear Mold Shrinkage 0.00300 - 0.0200 cm/cm0.00300 - 0.0200 in/inAverage value: 0.0145 cm/cm Grade Count:36
Melt Flow 0.300 - 58.0 g/10 min0.300 - 58.0 g/10 minAverage value: 12.6 g/10 min Grade Count:155
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 70.0 - 99.070.0 - 99.0Average value: 90.3 Grade Count:4
Hardness, Shore D 20.0 - 80.020.0 - 80.0Average value: 49.8 Grade Count:156
Tensile Strength, Ultimate 7.00 - 54.0 MPa1020 - 7830 psiAverage value: 27.2 MPa Grade Count:130
Tensile Strength, Yield 15.0 - 35.0 MPa2180 - 5080 psiAverage value: 22.2 MPa Grade Count:3
Elongation at Break 50.0 - 980 %50.0 - 980 %Average value: 407 % Grade Count:153
Elongation at Yield 10.0 - 74.0 %10.0 - 74.0 %Average value: 29.5 % Grade Count:14
Modulus of Elasticity 0.0500 - 1.00 GPa7.25 - 145 ksiAverage value: 0.266 GPa Grade Count:32
Tenacity 0.0120 - 0.0250 N/tex0.136 - 0.283 g/denierAverage value: 0.0187 N/tex Grade Count:10
Flexural Yield Strength 2.26 - 36.3 MPa327 - 5260 psiAverage value: 14.5 MPa Grade Count:29
Flexural Modulus 0.0150 - 1.18 GPa2.18 - 171 ksiAverage value: 0.248 GPa Grade Count:106
Compressive Modulus 0.00196 - 0.0350 GPa0.284 - 5.08 ksiAverage value: 0.0138 GPa Grade Count:4
Resilience 44.0 - 78.044.0 - 78.0Average value: 62.0 Grade Count:4
Izod Impact, Notched 0.686 J/cm - NB1.29 ft-lb/in - NBAverage value: 1.25 J/cm Grade Count:35
 0.0500 - 99.99 J/cm
@Temperature -40.0 - -40.0 °C
0.0937 - 187.3 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 0.907 J/cm Grade Count:14
 0.490332 - 980.567 J/cm
@Temperature -40.0 - -40.0 °C
0.918594 - 1837.00 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 0.907 J/cm Grade Count:16
 0.490332 - 980.567 J/cm
@Thickness 3.17 - 3.17 mm
0.918594 - 1837.00 ft-lb/in
@Thickness 0.125 - 0.125 in
Average value: 0.907 J/cm Grade Count:16
Izod Impact, Unnotched 1.1768 - 980.567 J/cm
@Temperature -40.0 - -23.0 °C
2.2046 - 1837.00 ft-lb/in
@Temperature -40.0 - -9.40 °F
Average value: 3.85 J/cm Grade Count:18
Izod Impact, Notched (ISO) 9.00 kJ/m² - NB4.28 ft-lb/in² - NBAverage value: 22.3 kJ/m² Grade Count:25
 5.00 kJ/m² - NB
@Temperature -40.0 - -20.0 °C
2.38 ft-lb/in² - NB
@Temperature -40.0 - -4.00 °F
Average value: 6.50 kJ/m² Grade Count:13
Charpy Impact Unnotched 0.600 J/cm² - NB
@Temperature -30.0 - -30.0 °C
2.86 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 0.600 J/cm² Grade Count:3
Charpy Impact, Notched 1.00 J/cm² - NB4.76 ft-lb/in² - NBAverage value: 2.90 J/cm² Grade Count:32
 0.600 J/cm² - NB
@Temperature -30.0 - -30.0 °C
2.86 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 1.27 J/cm² Grade Count:31
Tensile Impact Strength 179 - 233 kJ/m²85.2 - 111 ft-lb/in²Average value: 204 kJ/m² Grade Count:7
Tear Strength 40.0 - 280 kN/m228 - 1600 pliAverage value: 131 kN/m Grade Count:91
Graves Tear Strength 60.0 - 150 kN/m342 - 856 pliAverage value: 92.5 kN/m Grade Count:6
Taber Abrasion, mg/1000 Cycles 0.140 - 1200.140 - 120Average value: 42.7 Grade Count:34
Compression Set 50.0 - 60.0 %50.0 - 60.0 %Average value: 55.0 % Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+12 - 1.00e+15 ohm-cm1.00e+12 - 1.00e+15 ohm-cmAverage value: 3.52e+14 ohm-cm Grade Count:19
Surface Resistance 8.00e+10 - 1.00e+15 ohm8.00e+10 - 1.00e+15 ohmAverage value: 3.39e+14 ohm Grade Count:14
Dielectric Constant 3.30 - 20.03.30 - 20.0Average value: 4.84 Grade Count:15
Dielectric Strength 20.0 - 30.0 kV/mm508 - 762 kV/inAverage value: 22.1 kV/mm Grade Count:19
Dissipation Factor 0.00100 - 0.08100.00100 - 0.0810Average value: 0.0345 Grade Count:15
Comparative Tracking Index 600 V600 VAverage value: 600 V Grade Count:19
 
Thermal PropertiesMetricEnglishComments
CTE, linear 110 - 220 µm/m-°C61.1 - 122 µin/in-°FAverage value: 155 µm/m-°C Grade Count:22
CTE, linear, Transverse to Flow 110 - 220 µm/m-°C61.1 - 122 µin/in-°FAverage value: 151 µm/m-°C Grade Count:15
Melting Point 150 - 224 °C302 - 435 °FAverage value: 199 °C Grade Count:155
Maximum Service Temperature, Air 120 - 180 °C248 - 356 °FAverage value: 152 °C Grade Count:17
Deflection Temperature at 0.46 MPa (66 psi) 46.0 - 130 °C115 - 266 °FAverage value: 89.1 °C Grade Count:41
Deflection Temperature at 1.8 MPa (264 psi) 50.0 - 155 °C122 - 311 °FAverage value: 94.8 °C Grade Count:4
Vicat Softening Point 50.0 - 210 °C122 - 410 °FAverage value: 148 °C Grade Count:96
Brittleness Temperature -100 - -40.0 °C-148 - -40.0 °FAverage value: -62.1 °C Grade Count:77
Glass Transition Temp, Tg -78.0 - 28.0 °C-108 - 82.4 °FAverage value: -35.1 °C Grade Count:18
Flammability, UL94 HB - V-0HB - V-0Grade Count:26
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 180 - 220 °C356 - 428 °FAverage value: 200 °C Grade Count:18
Die Temperature 190 - 220 °C374 - 428 °FAverage value: 205 °C Grade Count:18
Melt Temperature 170 - 230 °C338 - 446 °FAverage value: 202 °C Grade Count:18
Drying Temperature 80.0 - 100 °C176 - 212 °FAverage value: 97.5 °C Grade Count:18
Moisture Content 0.0300 %0.0300 %Average value: 0.0300 % Grade Count:18
Injection Pressure 5.90 - 7.90 MPa856 - 1150 psiAverage value: 6.90 MPa Grade Count:18
Cycle Time - Injection 1.20 - 1.50 sec1.20 - 1.50 secAverage value: 1.35 sec Grade Count:18
Cycle Time - Cooling 10.0 - 20.0 sec10.0 - 20.0 secAverage value: 15.0 sec Grade Count:18

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polyester Thermoplastic Elastomer
Overview of materials for Thermoplastic Olefinic Elastomer (TPO)
Overview of materials for Styrenic Elastomer (TES)
Overview of materials for Thermoplastic Polyurethane, Elastomer, Polyester Grade
Overview of materials for Thermoplastic Elastomer, Melt-Processible Rubber

O5415 / 78502

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.