Physical Properties | Metric | English | Comments |
---|
Bulk Density | 0.640 g/cc @Temperature 23.0 °C | 0.0231 lb/in³ @Temperature 73.4 °F |
Density | 1.19 g/cc | 0.0430 lb/in³ |
Moisture Absorption at Equilibrium | 0.12 % @Temperature 23.0 °C | 0.12 % @Temperature 73.4 °F |
Water Absorption at Saturation | 0.40 % @Temperature 23.0 °C | 0.40 % @Temperature 73.4 °F |
Linear Mold Shrinkage | 0.0070 cm/cm @Pressure 50.0 MPa | 0.0070 in/in @Pressure 7250 psi |
Linear Mold Shrinkage, Flow | 0.0065 cm/cm @Pressure 50.0 MPa | 0.0065 in/in @Pressure 7250 psi |
Melt Flow | 8.5 g/10 min @Load 1.20 kg, Temperature 300 °C | 8.5 g/10 min @Load 2.65 lb, Temperature 572 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Ball Indentation Hardness | 103 MPa @Temperature 23.0 °C | 15000 psi @Temperature 73.4 °F |
Tensile Strength at Break | 60.0 MPa | 8700 psi |
Tensile Strength, Yield | 58.0 MPa | 8410 psi |
Elongation at Break | >= 50 % | >= 50 % |
| 120 % | 120 % |
Elongation at Yield | 5.7 % | 5.7 % |
Tensile Modulus | 2.20 GPa @Temperature 23.0 °C | 319 ksi @Temperature 73.4 °F |
Flexural Strength | 86.0 MPa | 12500 psi |
| 68.0 MPa @Strain 3.5 % | 9860 psi @Strain 3.5 % |
Flexural Modulus | 2.20 GPa @Temperature 23.0 °C | 319 ksi @Temperature 73.4 °F |
Flexural Strain at Break | 6.8 % | 6.8 % |
Izod Impact, Notched (ISO) | 45.0 kJ/m² @Thickness 3.00 mm, Temperature -30.0 °C | 21.4 ft-lb/in² @Thickness 0.118 in, Temperature -22.0 °F |
| 60.0 kJ/m² @Thickness 3.00 mm, Temperature 23.0 °C | 28.6 ft-lb/in² @Thickness 0.118 in, Temperature 73.4 °F |
Charpy Impact Unnotched | NB @Temperature 23.0 °C | NB @Temperature 73.4 °F |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
| NB @Temperature -60.0 °C | NB @Temperature -76.0 °F |
Charpy Impact, Notched | 5.00 J/cm² @Thickness 3.00 mm, Temperature -30.0 °C | 23.8 ft-lb/in² @Thickness 0.118 in, Temperature -22.0 °F |
| 6.00 J/cm² @Thickness 3.00 mm, Temperature 23.0 °C | 28.6 ft-lb/in² @Thickness 0.118 in, Temperature 73.4 °F |
Puncture Energy | 50.0 J @Temperature 23.0 °C | 36.9 ft-lb @Temperature 73.4 °F |
| 55.0 J @Temperature -30.0 °C | 40.6 ft-lb @Temperature -22.0 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+16 ohm-cm | 1.00e+16 ohm-cm |
Surface Resistance | 1.00e+16 ohm | 1.00e+16 ohm |
Dielectric Constant | 3.1 @Frequency 1e+6 Hz | 3.1 @Frequency 1e+6 Hz |
| 3.2 @Frequency 100 Hz | 3.2 @Frequency 100 Hz |
Dielectric Strength | 34.0 kV/mm @Thickness 1.00 mm | 864 kV/in @Thickness 0.0394 in |
Dissipation Factor | 0.0014 @Frequency 100 Hz | 0.0014 @Frequency 100 Hz |
| 0.0125 @Frequency 1e+6 Hz | 0.0125 @Frequency 1e+6 Hz |
Comparative Tracking Index | 100 V | 100 V |
| 225 V | 225 V |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 70.0 µm/m-°C @Temperature 23.0 - 55.0 °C | 38.9 µin/in-°F @Temperature 73.4 - 131 °F |
CTE, linear, Transverse to Flow | 70.0 µm/m-°C @Temperature 23.0 - 55.0 °C | 38.9 µin/in-°F @Temperature 73.4 - 131 °F |
Thermal Conductivity | 0.200 W/m-K | 1.39 BTU-in/hr-ft²-°F |
Hot Ball Pressure Test | 134 °C | 273 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 134 °C | 273 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 121 °C | 250 °F |
Vicat Softening Point | 141 °C @Load 5.10 kg | 286 °F @Load 11.2 lb |
| 143 °C @Load 5.10 kg | 289 °F @Load 11.2 lb |
Flammability, UL94 | HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
Flash Point | 450 °C | 842 °F |
Oxygen Index | 30 % | 30 % |
Glow Wire Ignition Temperature | 825 °C @Thickness 1.50 mm | 1520 °F @Thickness 0.0591 in |
| 825 °C @Thickness 2.00 mm | 1520 °F @Thickness 0.0787 in |
| 850 °C @Thickness 3.00 mm | 1560 °F @Thickness 0.118 in |
Glow Wire Flammability Index | 850 °C @Thickness 0.750 mm | 1560 °F @Thickness 0.0295 in |
| 875 °C @Thickness 1.50 mm | 1610 °F @Thickness 0.0591 in |
| 900 °C @Thickness 3.00 mm | 1650 °F @Thickness 0.118 in |
Ignition Temperature | 530 °C | 986 °F |
|
Processing Properties | Metric | English | Comments |
---|
Melt Temperature | 290 °C | 554 °F |
Mold Temperature | 80.0 °C | 176 °F |
Injection Velocity | 200 mm/sec | 7.87 in/sec |
|
Descriptive Properties |
---|
Burning Rate (mm/min) | passed, ISO 3795 |
Needle Flame Test (s) | 10 |
| 120 |
| 120 |
| 120 |
| 5 |
| 5 |
Puncture Maximum Force (N) | 4900 |
| 5800 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.