MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Lotte Advanced Materials Starex® TX-0550 MABS  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Transparent, Home Appliances, Toy

Information provided by Lotte Advanced Materials

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.09 g/cc1.09 g/ccNatural or representative color; ASTM D792
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0040 - 0.0080 in/in
@Thickness 0.126 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0040 - 0.0080 cm/cm
@Thickness 3.20 mm
0.0040 - 0.0080 in/in
@Thickness 0.126 in
ASTM D955
Melt Flow 25 g/10 min
@Load 10.0 kg,
Temperature 220 °C
25 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 110110ASTM D785
Tensile Strength at Break 43.1 MPa6250 psi50 mm/min; ASTM D638
Tensile Strength, Yield 41.2 MPa5970 psi5 mm/min; ASTM D638
Elongation at Break 25 %25 %5 mm/min; ASTM D638
Tensile Modulus 1.96 GPa284 ksi5 mm/min; ASTM D638
Flexural Strength 63.7 MPa9240 psi2.8 mm/min; ASTM D790
Flexural Modulus 2.06 GPa299 ksi2.8 mm/min; ASTM D790
Izod Impact, Notched  1.27 J/cm
@Thickness 6.35 mm
2.39 ft-lb/in
@Thickness 0.250 in
ASTM D256
 1.27 J/cm
@Thickness 3.17 mm
2.39 ft-lb/in
@Thickness 0.125 in
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 76.0 °C
@Thickness 6.40 mm
169 °F
@Thickness 0.252 in
ASTM D648
Vicat Softening Point 86.0 °C187 °FB/50; ISO R 306

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lotte Advanced Materials Starex® AS-0151 ABS, Unreinforced
Techmer ES HiFill FR® ASA FR-2A WT209
Lotte Advanced Materials Starex® GR4615 ABS/GF
Techmer ES HiFill FR® ASA FR-2 WT
Lotte Advanced Materials Starex® TX-0510T TRABS, Unreinforced

PLOTT9928 / 205791

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.