MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Alclad Aluminum 3003-H14
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 3000 Series Aluminum Alloy

Material Notes: Good weldability/formability and very good corrosion resistance lead to applications such as food and chemical handling, tanks, trim, litho sheet, pressure vessels, and piping.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes: Composition for AA 3003 (not Alclad 3003 specifically).
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A83003; Alclad 3003-H14; Alclad 3003-H14; Al3003-H14
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.73 g/cc0.0986 lb/in³For AA3003 (Not Alclad)
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 152 MPa22000 psiAA; Typical
 >= 130 MPa
@Thickness 0.229 - 12.7 mm
>= 18900 psi
@Thickness 0.00900 - 0.499 in
 >= 140 MPa
@Thickness 12.7 - 50.8 mm
>= 20300 psi
@Thickness 0.500 - 2.00 in
Tensile Strength, Yield 145 MPa21000 psiAA; Typical
 >= 110 MPa
@Thickness 0.229 - 12.7 mm
>= 16000 psi
@Thickness 0.00900 - 0.499 in
 >= 115 MPa
@Thickness 12.7 - 50.8 mm
>= 16700 psi
@Thickness 0.500 - 2.00 in
Elongation at Break  1.0 - 8.0 %
@Thickness 0.229 - 12.7 mm
1.0 - 8.0 %
@Thickness 0.00900 - 0.499 in
 8.0 %
@Thickness 1.59 mm
8.0 %
@Thickness 0.0625 in
AA; Typical
 10 %
@Thickness 12.7 - 50.8 mm
10 %
@Thickness 0.500 - 2.00 in
 16 %
@Diameter 12.7 mm
16 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 68.9 GPa10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Shear Strength 96.5 MPa14000 psiAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °FCommercial practice: 750 to 1100°F, higher temperatures used only for flash annealing.
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 96.7 - 99 %96.7 - 99 %As remainder
Copper, Cu 0.05 - 0.20 %0.05 - 0.20 %
Iron, Fe <= 0.70 %<= 0.70 %
Manganese, Mn 1.0 - 1.5 %1.0 - 1.5 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.60 %<= 0.60 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 3003-H14
Aluminum 6061-T6; 6061-T651
Alclad Aluminum 3003-H12
Alclad Aluminum 3003-H112
Alclad Aluminum 3003-O

MA3003AH14 / 8976

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.