MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Alcoa 2090-T83 Aluminum
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Aluminum-lithium alloy developed for high strength aerospace applications. The Al-Cu-Li alloy offers an 8 per cent density savings when compared with other aerospace alloys. Alloy 2090-T83 also has a 10 per cent higher elastic modulus. When coupled with the low density feature, this provides for unique weight saving benefits. Alloy 2090-T83 has strengths comparable with other high strength aluminum alloys and superior corrosion resistance. The alloy is also one of the most weldable aluminum products available.

Information provided by Alcoa.

Key Words: UNS A92090; Aluminium 2090-T83; AlLi; Aluminum Lithium Alloy; AA2090-T83
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.59 g/cc0.0936 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  >= 441 MPa
@Thickness 3.17 mm
>= 64000 psi
@Thickness 0.125 in
45° Direction
 >= 503 MPa
@Thickness 3.17 mm
>= 73000 psi
@Thickness 0.125 in
LT Direction
 >= 531 MPa
@Thickness 3.17 mm
>= 77000 psi
@Thickness 0.125 in
Longitudinal Direction
Tensile Strength, Yield  >= 386 MPa
@Thickness 3.17 mm
>= 56000 psi
@Thickness 0.125 in
45° Direction
 >= 455 MPa
@Thickness 3.17 mm
>= 66000 psi
@Thickness 0.125 in
LT Direction
 >= 483 MPa
@Thickness 3.17 mm
>= 70000 psi
@Thickness 0.125 in
Longitudinal Direction
Elongation at Break  >= 3.0 %
@Thickness 3.17 mm
>= 3.0 %
@Thickness 0.125 in
Longitudinal Direction
 >= 5.0 %
@Thickness 3.17 mm
>= 5.0 %
@Thickness 0.125 in
LT Direction
Modulus of Elasticity 79.3 GPa11500 ksi
Fatigue Strength  103 MPa
@# of Cycles 1.00e+7
15000 psi
@# of Cycles 1.00e+7
Notched (KT = 3)
 110 MPa
@# of Cycles 1.00e+6
16000 psi
@# of Cycles 1.00e+6
Notched (KT = 3)
 145 MPa
@# of Cycles 100000
21000 psi
@# of Cycles 100000
Notched (KT = 3)
 207 MPa
@# of Cycles 1.00e+7
30000 psi
@# of Cycles 1.00e+7
Smooth
 228 MPa
@# of Cycles 10000
33000 psi
@# of Cycles 10000
Notched (KT = 3)
 241 MPa
@# of Cycles 1.00e+6
35000 psi
@# of Cycles 1.00e+6
Smooth
 303 MPa
@# of Cycles 100000
44000 psi
@# of Cycles 100000
Smooth
 469 MPa
@# of Cycles 10000
68000 psi
@# of Cycles 10000
Smooth
Fracture Toughness 44.0 MPa-m½
@Thickness 3.17 mm
40.0 ksi-in½
@Thickness 0.125 in
KC, L-T
 
Thermal PropertiesMetricEnglishComments
CTE, linear 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
per Aluminum Association
Specific Heat Capacity 1.203 J/g-°C
@Temperature 100 °C
0.2875 BTU/lb-°F
@Temperature 212 °F
per Aluminum Association
Thermal Conductivity 88.0 W/m-K611 BTU-in/hr-ft²-°Fper Aluminum Association
Melting Point 560 - 650 °C1040 - 1200 °Fper Aluminum Association
Solidus 560 °C1040 °Fper Aluminum Association
Liquidus 650 °C1200 °Fper Aluminum Association
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 93.2 - 95.6 %93.2 - 95.6 %As remainder
Chromium, Cr <= 0.05 %<= 0.05 %
Copper, Cu 2.4 - 3.0 %2.4 - 3.0 %
Iron, Fe <= 0.12 %<= 0.12 %
Lithium, Li 1.9 - 2.6 %1.9 - 2.6 %
Magnesium, Mg <= 0.25 %<= 0.25 %
Manganese, Mn <= 0.05 %<= 0.05 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.10 %<= 0.10 %
Titanium, Ti <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.10 %<= 0.10 %
Zirconium, Zr 0.08 - 0.15 %0.08 - 0.15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 2090-T86
Aluminum 8090-T8x
Aluminum 7034-T6
Aluminum 8090-T8151
Aluminum 2090-T83

NALCOA25 / 176079

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.