MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Riteflex® 677 TPC, Unfilled
Categories: Polymer; Thermoplastic; Polyester, TP; Polyester Thermoplastic Elastomer

Material Notes: Riteflex 677 is a thermoplastic polyester elastomer with nominal hardness of 77 shore D and high modulus.

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.29 g/cc1.29 g/ccASTM D792
Density 1.27 g/cc0.0459 lb/in³ISO 1183
Water Absorption 0.10 %
@Temperature 22.8 °C
0.10 %
@Temperature 73.0 °F
24hr immersion; ASTM D570
Viscosity 461200 cP461200 cP
Linear Mold Shrinkage, Flow 0.020 cm/cm0.020 in/inASTM D955
 0.018 - 0.022 cm/cm0.018 - 0.022 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.017 - 0.022 cm/cm0.017 - 0.022 in/inISO 294-4
Melt Flow 12 - 16 g/10 min12 - 16 g/10 minASTM D1238
 15 g/10 min
@Load 2.16 kg,
Temperature 240 °C
15 g/10 min
@Load 4.76 lb,
Temperature 464 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 757515 sec; ISO 868
 7777ASTM D2240
Tensile Strength at Break 42.0 MPa6090 psi50mm/min; ISO 527-2/1A
Tensile Strength, Yield 33.0 MPa4790 psi50mm/min; ISO 527-2/1A
 34.5 MPa5000 psiASTM D638
Tensile Stress at Strain  26.0 MPa
@Strain 50 %
3770 psi
@Strain 50 %
ISO 527-2/1A
 26.0 MPa
@Strain 50 %
3770 psi
@Strain 50 %
ISO 727-1/2
 32.0 MPa
@Strain 5.0 %
4640 psi
@Strain 5.0 %
ISO 527-1/2
 36.0 MPa
@Strain 10 %
5220 psi
@Strain 10 %
ISO 527-1/2
Elongation at Break >= 50 %>= 50 %
 310 %310 %ASTM D638
 350 %350 %50mm/min; ISO 527-2/1A
Elongation at Yield 15 %15 %50mm/min; ISO 527-2/1A
Tensile Modulus 0.689 GPa100 ksiASTM D638
 0.750 GPa109 ksi50mm/min; ISO 527-2/1A
Flexural Strength 30.0 MPa4350 psiISO 178
 23.0 MPa
@Strain 3.5 %
3340 psi
@Strain 3.5 %
ISO 178
Flexural Modulus 0.650 GPa94.3 ksiISO 178
 0.689 GPa100 ksiASTM D790
 2.50 GPa
@Temperature -40.0 °C
363 ksi
@Temperature -40.0 °F
ISO 178
Resilience 4040Bayshore, %; ASTM D2632
 4040Bayshore, %
Izod Impact, Notched 2.19 J/cm4.10 ft-lb/inASTM D256
 0.374 J/cm
@Temperature -40.0 °C
0.700 ft-lb/in
@Temperature -40.0 °F
ASTM D256
Izod Impact, Unnotched NBNBASTM D256
Izod Impact, Notched (ISO) 4.70 kJ/m²2.24 ft-lb/in²ISO 180
 8.50 kJ/m²4.04 ft-lb/in²ISO 180/1A
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 180/1U
Charpy Impact Unnotched 7.10 J/cm²33.8 ft-lb/in²ISO 179/1eU
 0.450 J/cm²
@Temperature -30.0 °C
2.14 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched 0.940 J/cm²4.47 ft-lb/in²ISO 179/1eA
Tear Strength 250 kN/m1430 pliISO 34-1
 358 kN/m2040 pliASTM D624
 362.0 kN/m2065 pliASTM D1004
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 5.00e+14 ohm-cm5.00e+14 ohm-cmASTM D257
 4.00e+16 ohm-cm4.00e+16 ohm-cmIEC 60093
Surface Resistance 2.00e+17 ohm2.00e+17 ohmIEC 60093
Dielectric Constant 3.3
@Frequency 1e+6 Hz
3.3
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 15.0 kV/mm380 kV/inshort term; ASTM D149
 16.0 kV/mm406 kV/inIEC 60243-1
Dissipation Factor 0.040
@Frequency 1e+6 Hz
0.040
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index >= 600 V>= 600 VASTM D3638
 >= 600 V>= 600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 140 µm/m-°C77.8 µin/in-°FISO 11359-2
Melting Point 217 °C423 °FASTM D3418
 218 °C424 °F10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 109 °C228 °FISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi) 51.0 °C124 °FISO 75-1, -2
Flammability, UL94 HBHB
 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 55.0 °C68.0 - 131 °Fcavity
 235 - 260 °C455 - 500 °Fhot runner
Feed Temperature 230 - 240 °C446 - 464 °F
Zone 1 230 - 240 °C446 - 464 °F
Zone 2 235 - 250 °C455 - 482 °F
Zone 3 235 - 250 °C455 - 482 °F
Zone 4 240 - 260 °C464 - 500 °F
Die Temperature 240 - 260 °C464 - 500 °F
Melt Temperature 235 - 260 °C455 - 500 °F
Drying Temperature 100 - 110 °C212 - 230 °F
Dry Time 4.00 hour4.00 hour
Moisture Content <= 0.050 %<= 0.050 %
 
Compliance PropertiesMetricEnglishComments
FDA NoNo
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Riteflex® 663 TPC, Unfilled
Celanese Riteflex® UV655M TPC, Unfilled
Celanese Riteflex® XFR 655 TPC, Unfilled
Celanese Riteflex® 672 TPC, Unfilled
Celanese Riteflex® 830 TPC, Unfilled

PHCQ457 / 178912

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.