MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Nylon 66, 10% Mineral Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 10% Mineral Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 66, 10% Mineral Filled". Specific grades with primary filler content between 5% and 14% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.10 - 1.60 g/cc0.0397 - 0.0578 lb/in³Average value: 1.26 g/cc Grade Count:9
Water Absorption 0.600 - 2.30 %0.600 - 2.30 %Average value: 1.34 % Grade Count:6
Water Absorption at Saturation 5.00 - 8.00 %5.00 - 8.00 %Average value: 6.33 % Grade Count:3
Linear Mold Shrinkage 0.00200 - 0.0250 cm/cm0.00200 - 0.0250 in/inAverage value: 0.0143 cm/cm Grade Count:7
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 48.0 - 90.0 MPa6960 - 13100 psiAverage value: 75.6 MPa Grade Count:5
Tensile Strength, Yield 78.5 - 93.1 MPa11400 - 13500 psiAverage value: 85.0 MPa Grade Count:3
Elongation at Break 1.00 - 14.0 %1.00 - 14.0 %Average value: 5.58 % Grade Count:6
Modulus of Elasticity 3.10 - 7.50 GPa450 - 1090 ksiAverage value: 4.54 GPa Grade Count:5
Flexural Yield Strength 90.0 - 138 MPa13100 - 20000 psiAverage value: 112 MPa Grade Count:6
Flexural Modulus 2.30 - 6.89 GPa334 - 1000 ksiAverage value: 4.40 GPa Grade Count:5
Izod Impact, Notched 0.210 - 0.490 J/cm0.393 - 0.919 ft-lb/inAverage value: 0.399 J/cm Grade Count:4
Izod Impact, Notched (ISO) 3.00 - 4.00 kJ/m²
@Temperature -40.0 - -30.0 °C
1.43 - 1.90 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 3.50 kJ/m² Grade Count:1
Izod Impact, Unnotched (ISO) 27.0 - 27.0 kJ/m²
@Temperature -30.0 - -30.0 °C
12.8 - 12.8 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 27.0 kJ/m² Grade Count:1
Charpy Impact Unnotched 2.00 J/cm² - NB9.52 ft-lb/in² - NBAverage value: 2.50 J/cm² Grade Count:4
 3.00 J/cm² - NB
@Temperature -40.0 - -30.0 °C
14.3 ft-lb/in² - NB
@Temperature -40.0 - -22.0 °F
Average value: 3.00 J/cm² Grade Count:2
Charpy Impact, Notched 0.130 - 0.530 J/cm²0.619 - 2.52 ft-lb/in²Average value: 0.345 J/cm² Grade Count:4
 0.200 - 0.460 J/cm²
@Temperature -40.0 - -30.0 °C
0.952 - 2.19 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 0.347 J/cm² Grade Count:3
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+8 - 1.00e+15 ohm-cm1.00e+8 - 1.00e+15 ohm-cmAverage value: 8.00e+14 ohm-cm Grade Count:5
Comparative Tracking Index 550 - 600 V550 - 600 VAverage value: 583 V Grade Count:3
 
Thermal PropertiesMetricEnglishComments
CTE, linear  35.0 - 35.0 µm/m-°C
@Temperature 35.0 - 55.0 °C
19.4 - 19.4 µin/in-°F
@Temperature 95.0 - 131 °F
Average value: 35.0 µm/m-°C Grade Count:1
 35.0 - 35.0 µm/m-°C
@Thickness 2.00 - 2.00 mm
19.4 - 19.4 µin/in-°F
@Thickness 0.0787 - 0.0787 in
Average value: 35.0 µm/m-°C Grade Count:1
Deflection Temperature at 0.46 MPa (66 psi) 200 - 252 °C392 - 485 °FAverage value: 235 °C Grade Count:7
Deflection Temperature at 1.8 MPa (264 psi) 115 - 250 °C239 - 482 °FAverage value: 201 °C Grade Count:5
Flammability, UL94 HB - V-0HB - V-0Grade Count:4
 
Processing PropertiesMetricEnglishComments
Melt Temperature 260 - 300 °C500 - 572 °FAverage value: 277 °C Grade Count:3
Mold Temperature 60.0 - 107 °C140 - 225 °FAverage value: 85.0 °C Grade Count:3
Drying Temperature 75.0 - 107 °C167 - 225 °FAverage value: 91.7 °C Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 66, 20% Mineral Filled
Overview of materials for Nylon 66, 30% Mineral Filled
Overview of materials for Nylon 66, 40% Mineral Filled
BASF Ultramid® A3EG3 15% Glass Filled PA66 (Dry)
BASF Ultramid® A3EG3 15% Glass Filled PA66 (Conditioned)

O2531 / 78028

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.