MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

American White Ash Wood
Categories: Wood and Natural Products; Wood; Hardwood

Material Notes: Ring-Porous Hardwood. Least easy to work with hand tools. Excellent shaping, very good planing, very good steam bending. Data is based on small, clear, air-dried samples unless specified.

Property values marked by an asterisk (*) have been taken from an unusually old reference source.

Key Words: Fraxinus americana; Lumber, Timber
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.550 g/cc0.0199 lb/in³Oven Dry Weight/Unseasoned Volume
 0.769 g/cc0.0278 lb/in³Unseasoned*
Cell Length 1.20 mm0.0472 inMature Wood
 
Mechanical PropertiesMetricEnglishComments
Hardness, Wood Indentation 4000 N899 lb (f)Side. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 4400 N989 lb (f)End. Force required to imbed a 0.444 inch steel ball to one-half its diameter
 5900 N1330 lb (f)Side
Tensile Strength, Ultimate 4.27 MPa620 psiPerpendicular to Grain*
 6.50 MPa943 psiPerpendicular to Grain
Modulus of Rupture 0.0627 GPa9.10 ksiStatic Bending*
 0.106 GPa15.4 ksiIn Bending
Flexural Yield Strength 33.8 MPa4900 psiFiber Stress at Elastic Limit; Static Bending*
 61.4 MPa8910 psiBending stress at proportional limit
Flexural Modulus 9.31 GPa1350 ksiStatic Bending*
 12.0 - 12.4 GPa1740 - 1800 ksiIn Bending
Compressive Strength 5.52 MPa800 psiPerpendicular to Grain*
 8.00 MPa1160 psiPerpendicular to Grain
 22.3 MPa3230 psiParallel to Grain*
 26.2 MPa3800 psiMax Crushing Strength Parallel to Grain*
 51.0 MPa7400 psiParallel to Grain
Poissons Ratio 0.0510.051µTL, 12% Moisture Content
 0.0590.059µRL, 12% Moisture Content
 0.360.36µTR, 12% Moisture Content
 0.3710.371µLR, 12% Moisture Content
 0.440.44µLT, 12% Moisture Content
 0.6840.684µRT, 12% Moisture Content
Shear Strength 8.69 MPa1260 psiParallel to Grain*
 13.4 MPa1940 psiOrientation Unknown
Impact 5.05.0in-lb/in³; Work to Elastic Limit; Unseasoned Sample; Impact Bending*
 1170011700psi; Fiber Stress at Elastic Limit; Unseasoned Sample; Impact Bending*
Work to Elastic Limit 0.00710 J/cm³1.03 in-lb/in³Static Bending*
Work to Maximum Load 0.0924 J/cm³13.4 in-lb/in³Static Bending*
Cleavage 58.0 kN/m331 lb/inRadial surface of failure, Unseasoned*
 61.0 kN/m348 lb/inTangential surface of failure, Unseasoned*
 
Thermal PropertiesMetricEnglishComments
CTE, linear 9.50 µm/m-°C
@Temperature 20.0 °C
5.28 µin/in-°F
@Temperature 68.0 °F
Axial. Typical value for Ash.
Thermal Conductivity 0.141 W/m-K0.980 BTU-in/hr-ft²-°FOven Dry
 0.173 W/m-K1.20 BTU-in/hr-ft²-°F12% Moisture Content
Shrinkage 4.9 %4.9 %Radial; Unseasoned to Oven Dry*
 7.9 %7.9 %Tangential; Unseasoned to Oven Dry*
 13.2 %13.2 %Volumetric; Unseasoned to Oven Dry*

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 5086-H116; 5086-H32
Aluminum 5052-H32
Aluminum 5083-H116; 5083-H321
American Ash Wood
European Ash Wood

PTSAM / 71296

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.