MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

RheTech Products UVFT3082-74 Thermoplastic Polyolefin, 135K Flexural Modulus, UV Stabilized, Exterior DX9 Black
Categories: Polymer; Thermoplastic; Polyolefin

Material Notes: Applications:
  • Step pads
  • Hitch pads
  • Exterior trim

Injection molding conditions reported in table.

Information provided by RheTech Products.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.900 g/cc
@Temperature 23.0 °C
0.900 g/cc
@Temperature 73.4 °F
23/23°C; ASTM D792
Linear Mold Shrinkage 0.0137 cm/cm0.0137 in/inASTM D955
Melt Flow 18 g/10 min
@Load 2.16 kg,
Temperature 230 °C
18 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6565ASTM D2240
Tensile Strength at Break 17.9 MPa2600 psi2 in/min; ASTM D638
Flexural Modulus 0.931 GPa135 ksiTangent; ASTM D790
Izod Impact, Notched 8.01 J/cm
@Temperature 23.0 °C
15.0 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Gardner Impact 22.6 J16.7 ft-lbASTM D5420
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 76.7 °C170 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 48.9 °C120 °FASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 188 - 216 °C370 - 420 °F
Middle Barrel Temperature 193 - 221 °C380 - 430 °F
Front Barrel Temperature 199 - 227 °C390 - 440 °F
Nozzle Temperature 204 - 216 °C400 - 420 °F
Mold Temperature 26.7 - 48.9 °C80.0 - 120 °F
Drying Temperature 65.6 - 82.2 °C150 - 180 °F
Dry Time 1 - 2 hour1 - 2 hour
Moisture Content <= 0.050 %<= 0.050 %Recommended
Injection Pressure 2.76 - 10.3 MPa400 - 1500 psi
Hold Pressure 2.07 - 8.27 MPa300 - 1200 psi
Back Pressure 0.345 - 1.03 MPa50.0 - 150 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RheTech Products FT3080-727UV Thermoplastic Polyolefin, UV Stabilized, G01 Black
RheTech Products FT5250-650UV Thermoplastic Polyolefin, UV Stabilized, Exterior 848 Black
RheTech Products FT4900-74UV Thermoplastic Polyolefin, UV Stabilized, Exterior DX9 Black
RheTech Products FT4900-01UV Thermoplastic Polyolefin, UV Stabilized, Black
RheTech Products HP800-706UV 20% Talc Reinforced High Performance Polypropylene Copolymer, Scratch Resistant, UV Stabilized, Impact Modified, SWB White

PRHET356 / 65924

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.